| HS Code | 346514 |
| Polymer Type | High Density Polyethylene |
| Density | 0.951 g/cm3 |
| Melt Flow Rate 190 C 2 16 Kg | 0.8 g/10 min |
| Tensile Strength At Yield | 28 MPa |
| Tensile Elongation At Break | >500% |
| Flexural Modulus | 1200 MPa |
| Izod Notched Impact Strength | 50 J/m |
| Vicat Softening Temperature | 125 °C |
| Heat Deflection Temperature 0 45 Mpa | 70 °C |
| Shore D Hardness | 65 |
| Environmental Stress Crack Resistance Escr | >1000 h |
| Brittleness Temperature | < -70 °C |
| Melt Density | 0.760 g/cm3 |
As an accredited SCG Chemicals HDPE H511W factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | SCG Chemicals HDPE H511W is supplied in 25 kg polyethylene-lined woven bags, typically stacked 40 bags per pallet (1,000 kg). |
| Container Loading (20′ FCL) | 20′ FCL loaded with SCG Chemicals HDPE H511W high-density polyethylene pellets in 25 kg bags, palletized, shrink-wrapped, and securely stowed. |
| Shipping | SCG Chemicals HDPE H511W is a non-hazardous high-density polyethylene resin in pellet form. It ships in moisture-resistant bags or bulk containers as general cargo. Keep dry, avoid heat, sunlight, and ignition sources. No UN dangerous goods classification is required; standard road, rail, sea, or air freight applies. Store in original packaging. |
| Storage | Store SCG Chemicals HDPE H511W in a cool, dry, well-ventilated warehouse, away from direct sunlight, heat, flames, and strong oxidizers. Keep original bags or packaging closed and intact, on pallets off the floor, to prevent moisture, dust, and contamination. Avoid prolonged UV exposure and excessive stacking. Use first-in, first-out stock rotation. Store separately from food, feed, and incompatible materials. |
| Shelf Life | SCG Chemicals HDPE H511W shelf life: 24 months from manufacture when stored sealed, dry, cool, and away from direct sunlight. |
SCG Chemicals HDPE H511W is specified for extrusion blow-moulded containers where environmental stress crack resistance, melt strength and pinch-off weld integrity are principal process requirements. The grade is processed on conventional accumulator-head and continuous-extrusion shuttle machines; it is not intended for injection moulding or rotomoulding. Typical melt flow rate is 0.25–0.45 g/10 min at 190 °C under 2.16 kg load in accordance with ISO 1133-1:2022, and density is 0.951–0.956 g/cm³ per ISO 1183-1:2019.
In 20 L to 25 L extrusion blow-moulded jerry cans intended for UN-certified transport of liquid dangerous goods, H511W is processed on accumulator-head shuttle machines with a 75 mm extruder, 24:1 L/D barrier screw, grooved feed section and 2.5 L accumulator head. Barrel zone set points from feed to head are typically 170 °C, 180 °C, 190 °C, 195 °C, 200 °C, die 195 °C; head pressure remains between 18 MPa and 24 MPa. The melt temperature window for consistent pinch-off weld strength is ±5 °C around 190 °C. A 5 °C upward excursion increases parison drawdown by 8–12% and produces thin sidewall bands; a 5 °C downward excursion raises head pressure by 10–15% and may initiate shark-skin at the die exit. Ten-point radial parison programming is mandatory for a 250 g to 320 g jerry can; die gap is maintained at 1.8–2.5 mm, and blow air pressure is 0.6–0.8 MPa. Mould temperature is held at 10–15 °C with cycle times of 55–75 s.
Qualification for UN dangerous goods packagings is based on the drop test described in the UN Model Regulations 6.1.5.3.5 and the leakproofness test in 6.1.5.4. For packaging group II liquids, the filled container is conditioned to -18 °C and dropped from 1.2 m; acceptance requires no rupture and no leakage after closure verification. ESCR is screened in accordance with ASTM D1693-15 Condition B using 10% Igepal CO-630 by volume in water at 50 °C; containers for aggressive aqueous chemicals are accepted only when the notched specimen exceeds 100 h without crack propagation. Stack compression is assessed at 40 °C for 28 days under a load equivalent to 4.5 m of filled warehouse stacking; creep deformation above 2.5% of nominal height is treated as a practical rejection limit.
When the jerry can is used for flammable liquids with flash point below 60 °C, antistatic masterbatch at 2–4 wt% is incorporated after drying at 80 °C for 2 h. In tropical storage with relative humidity above 80%, surface condensation on virgin pellets causes intermittent splay and pinhole defects; a dehumidifying hopper dryer set to 60 °C for 1 h is used solely to remove surface moisture, because H511W is not hygroscopic. The primary incompatibility is with excessive levels of process aid or lubricant that reduce interlayer fusion at the pinch-off seam; silicone-based external mould release compounds are not permitted on the flash spreader plate due to weld-line contamination.
| Performance property | Standard designation | Typical acceptance window / condition |
|---|---|---|
| Melt flow rate | ISO 1133-1:2022 | 0.25–0.45 g/10 min at 190 °C / 2.16 kg |
| Density | ISO 1183-1:2019 | 0.951–0.956 g/cm³ |
| Environmental stress crack resistance | ASTM D1693-15 Condition B | Minimum 100 h in 10% Igepal CO-630 at 50 °C |
| Tensile yield stress | ISO 527-2:2012 | 24–28 MPa |
| Drop impact resistance | ASTM D2463-15 | No rupture at -18 °C for 1.2 m packaging group II drop |
| Chemical resistance screening | ASTM D543-14 | Mass change below 1.0% and tensile retention above 80% |
Closed-loop mould temperature control becomes the dominant constraint when a 1 L HDPE bottle for household detergent is produced at 0.6–0.8 mm body wall thickness on a two-cavity shuttle machine. Die swell variation across the parison circumference is held below 5% by maintaining melt temperature at 180–195 °C and by using a die gap of 0.8–1.2 mm. A 38 g bottle with 28/410 neck finish is blown at 0.55–0.7 MPa, with a pre-blow delay of 0.2–0.5 s and mould temperature 12–18 °C. Top-load strength is measured under ASTM D2659-16; an empty bottle should not buckle below 45 N at 23 °C. Drop impact resistance is screened by ASTM D2463-15 at -10 °C, with acceptance at 1.0 m for the filled bottle. High-output runs exceeding 18 shots/min per cavity without melt-pressure compensation generate wall-thickness drift at the bottle shoulder, which leads to cap thread ovality outside 0.5 mm.
When formulated organophosphate emulsifiable concentrates are packaged at 5 L to 10 L scale, the container wall must resist both chemical attack and dimensional deformation at warehouse temperatures up to 40 °C. H511W is used for paraffinic oil-based emulsion formulations; it is not qualified as a monolayer solution for aromatic solvent fractions above 10 wt% xylene or toluene, because published permeation data for this specific configuration is limited and the standard qualification route is mass-change screening under ASTM D543-14 at 40 °C for 14 days rather than assumed barrier performance. Accepted bottles show mass change below 1.0% and tensile yield retention above 80% per ISO 527-2:2012. Where the formulation contains more than 10 wt% aromatic hydrocarbon, the container must be surface-fluorinated or coextruded with a polyamide barrier layer; otherwise panel deformation and environmental stress cracking occur at the bottom pinch-off and handle flash junctions.
The pinch-off seam at the base is a critical stress concentrator; flash thickness after trimming must remain between 0.8 mm and 1.2 mm. A thinner flash section concentrates bulk strain at the weld line and accelerates cracking in the presence of wetting agents. On a 1.5 kg accumulator-head machine producing 5 L bottles, extrusion temperature is 185–200 °C and blow air is 0.65 MPa. Post-mould cooling fixtures hold the handle and neck in fixed geometry for 20–30 s after demoulding to prevent handle distortion above 1.5 mm.
For 30 L three-layer jerricans containing post-consumer HDPE recyclate, H511W is allocated to the virgin cap layers because its melt strength tolerates the higher pressure drop through a five-layer extrusion die. The layer ratio is set at 20% virgin inner, 60% PCR core, 20% virgin outer by thickness. Viscosity mismatch between H511W and the PCR component must be kept within 0.8–1.2 at apparent shear rate 100 s⁻¹; outside this band, interfacial migration produces wavy layer boundaries and reduces top-load resistance by 15–20%. Layer thickness distribution is checked by ultrasonic gauge at 12 points around the circumference; variation greater than 20% between the thinnest and thickest virgin layer is a process rejection condition. Die temperature is raised to 200–210 °C at the outer annulus while core melt is held at 195 °C, and the die gap is 2.2–3.0 mm. The coextruded parison is inflated at 0.7 MPa with a 10-point programmer biased toward the corner regions to maintain minimum 1.2 mm wall thickness at the base chimes.
Compliance for recycled-content packaging is documented under EU Packaging and Packaging Waste Directive 94/62/EC and, where relevant, EU Regulation 2022/1616 for food contact recycled plastics; for non-food industrial jerricans, PCR quality is limited by melt filtration at 200–300 µm mesh to restrict gel specks. The conversion line operates under a nitrogen purge of 0.1 m³/h at the feed throat to reduce oxidative degradation of the recyclate. Published data for H511W in tri-layer PCR structures is limited, so start-up runs require adjustment of die temperature profile and PCR input lot screening before continuous production.
| Container format | Machine and screw configuration | Melt temperature | Die gap | Blow air | Mould temperature | Cycle time |
|---|---|---|---|---|---|---|
| 20–25 L UN jerry can | 75 mm, 24:1 L/D, 2.5 L accumulator head | 180–205 °C | 1.8–2.5 mm | 0.6–0.8 MPa | 10–15 °C | 55–75 s |
| 1 L detergent bottle | 60 mm, 20:1 L/D, two-cavity shuttle | 180–195 °C | 0.8–1.2 mm | 0.55–0.7 MPa | 12–18 °C | 8–12 s |
| 30 L three-layer PCR jerrican | 90 mm, 26:1 L/D, five-layer die | Outer 200–210 °C, core 195 °C | 2.2–3.0 mm | 0.7 MPa | 15 °C | 90–120 s |
| 5 L lubricant bottle | 70 mm, 24:1 L/D, dual-station accumulator head | 170–190 °C | 1.5–2.0 mm | 0.6 MPa | 12 °C | 35–45 s |
Under sustained contact with ethoxylated non-ionic surfactants at 45 °C, high-molecular-weight HDPE blow moulding grades develop environmental stress cracking through tie-molecule scission; H511W is specified in 200 mL to 500 mL cosmetic bottles where the formulation contains less than 5.0 wt% non-ionic surfactant and no free aromatic solvent. The bottle wall thickness is 0.5–0.7 mm, and ESCR is qualified by ASTM D1693-15 Condition B with a minimum 150 h crack-free interval for stock solutions adjusted to pH 5–7. Filled-bottle top-load is measured at 23 °C under ASTM D2659-16; oval containers below 150 N after 7 days contact with the formulation are rejected because sidewall creep indicates plasticisation. The recommended processing route is a 60 mm extruder with 20:1 L/D screw, single station, two-cavity tooling, melt temperature 175–190 °C, and blow pressure 0.5–0.65 MPa. Mould cooling is set to 12 °C to limit sink marks at the thread neck. Hot filling above 65 °C is outside the continuous service range for HDPE; short-term exposure to 80 °C for 30 s during sanitising is tolerated but reduces top-load by 5–10% in subsequent stacking.
The in-line leak test station for 5 L closed-head lubricant bottles imposes a 0.3 bar internal air pressure differential across the parison pinch-off seam and the neck closure seat. The bottle is expected to maintain pressure within 0.02 bar over a 5 s dwell; any leakage at the bottom pinch-off, flash trim area, or handle junction forces immediate production hold. On a dual-station accumulator-head machine producing 80 g bottles at 170–190 °C melt temperature, the bottom flash after trimming is held at 0.8–1.2 mm to preserve weld-line strength. Too thin a flash, below 0.6 mm, correlates with channel leaks along the pinch-off and is caused by excessive parison programming at the bottom section. Drop impact is screened under ASTM D2463-15 at -5 °C with the bottle filled to nominal volume; a 0.8 m drop without rupture is the minimum acceptance criterion for lubricant shelf packaging. Because motor oil is a purely organic liquid, ESCR is less limiting than impact and leakage; nevertheless, the cap thread area is dimensionally checked with a go/no-go gauge to 0.3 mm ovality and the neck sealing surface is inspected for flash intrusion exceeding 0.1 mm.
Competitive SCG Chemicals HDPE H511W prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
SCG Chemicals HDPE H511W is a blow-molding grade of high-density polyethylene supplied as pellets. The resin has a nominal density of 0.951 g/cm³ when tested in accordance with ASTM D1505 and a melt flow rate of 0.30 g/10 min at 190 °C under 2.16 kg load in accordance with ASTM D1238. The low melt flow rate places the material in the high-molecular-weight segment of HDPE used for extrusion blow molding, where parison melt strength and environmental stress crack resistance are prioritized over cycle-time-driven melt flow. On continuous extrusion blow-molding equipment with die diameters of 10–150 mm, the grade is used to produce containers with capacities typically between 0.1 L and 10 L. Because the melt flow rate is below 1 g/10 min, H511W is not intended for thin-wall injection molding; high-flow HDPE grades with melt flow rates of 5–30 g/10 min are required for multi-cavity injection tools with wall sections below 1.0 mm.
The low melt index corresponds to elevated melt viscosity at low shear rates, which is a functional requirement for a vertically suspended parison that must retain a uniform diameter during mold closing. While the published datasheet does not list weight-average molecular weight or molecular weight distribution, the standardized melt flow rate and density values define the general class of high-molecular-weight blow-molding HDPE. Capillary rheometry under ASTM D3835 can be used to characterize shear viscosity at shear rates between 10 s⁻¹ and 1000 s⁻¹; H511W-specific viscosity curves are available from the manufacturer on request.
The following table lists published typical values for natural H511W pellets. The values are determined at 23 °C unless otherwise noted and represent nominal results from the manufacturer’s technical data; they do not replace lot-specific certificates of analysis.
| Property | Test Method | Typical Value |
|---|---|---|
| Density | ASTM D1505 | 0.951 g/cm³ |
| Melt flow rate, 190 °C/2.16 kg | ASTM D1238 | 0.30 g/10 min |
| Tensile strength at yield | ASTM D638 | 26 MPa |
| Elongation at break | ASTM D638 | >600% |
| Flexural modulus | ASTM D790 | 1,100 MPa |
| Environmental stress crack resistance, F50, 100% Igepal, 50 °C | ASTM D1693 Condition B | >600 h |
| Vicat softening temperature, 10 N | ASTM D1525 | 125 °C |
| Hardness, Shore D | ASTM D2240 | 63 |
The combination of flexural modulus near 1,100 MPa and an ESCR value above 600 h under 100% Igepal at 50 °C is a selection criterion for detergent and lubricant packages. The ESCR result provides a standardized measure of resistance to slow crack growth when the container wall is stressed by aggressive liquid contact. Density at 0.951 g/cm³ is moderately lower than high-density HDPE grades engineered for maximum shear modulus, indicating that H511W trades some top-load rigidity for improved stress crack resistance.
Continuous extrusion blow molding of H511W is normally conducted on single-screw extruders with screw diameters from 45 mm to 90 mm and length-to-diameter ratios from 24:1 to 30:1. Barrel profiles are typically ramped from 170 °C in the feed zone to 210 °C in the metering zone, while the die head is maintained between 190 °C and 220 °C. The low melt flow rate of 0.30 g/10 min produces a comparatively high shear viscosity; as a result, screw speed is typically constrained to 40–70 rpm on a 60 mm, 24:1 L/D production extruder to prevent viscous heating from driving melt temperature above 220 °C. If screw speed exceeds 80 rpm, the residence time distribution narrows but the surface temperature at the screw root can exceed the bulk melt setpoint by 10–20 °C. This temperature overshoot can produce gel bodies or surface pitting when the melt contacts the die lip at elevated temperature. Die head pressure on such equipment generally remains between 10 MPa and 30 MPa; H511W-specific pressure-drop curves are limited in public literature.
Melt temperature should be measured at the die entrance with a thermocouple immersion probe. Because HDPE exhibits shear thinning, raising screw speed does not produce a linear decrease in viscosity across all shear rates. The grade is best processed in a controlled envelope rather than at maximum throughput, particularly when the extruder is coupled to a single-station shuttle blow molder with clamped mold tonnage between 20 t and 80 t.
In multi-cavity continuous blow molding, the low melt flow rate of H511W permits a vertically suspended parison to resist sag over drop lengths of 150–400 mm when the melt temperature is kept between 190 °C and 210 °C. Die swell values for high-molecular-weight HDPE are generally in the range of 1.3–1.8; actual values depend on die land length, melt temperature, and parison shear history. Parison programming is used to vary the die gap from 0.8 mm to 2.5 mm along the preform length, generating a programmed wall thickness distribution that compensates for higher wall thinning near the pinch-off and shoulder regions. Published data for H511W-specific die swell as a function of die gap is limited.
Thermo-oxidative degradation of HDPE accelerates when the melt is exposed to oxygen at temperatures above 220 °C. For H511W, prolonged residence time at 230 °C or above can reduce molecular weight through chain scission; the practical indicator is a drop in die head pressure and a loss of parison melt strength, followed by surface defects in the finished container. The upper melt temperature limit is therefore 220 °C, with a recommended target of 195–210 °C. If start-up interruptions force residence times beyond 15 min, the extruder should be purged with HDPE until the melt at the die lip clears. Moisture absorption by the pellet surface is not a primary concern at ambient relative humidity below 60%; if sacks are opened in humid conditions above 60% and condensation is visible, the pellets should be dried at 80 °C for 2 h before extrusion. The material is not compatible with strong oxidizing media at melt temperature; contact with free radical initiators or copper ions can accelerate molecular weight loss.
Containers made from H511W are specified for household chemical formulations, lubricating oils, and personal-care surfactants. The standardized ESCR result above 600 h supports use with detergent concentrates and hydrocarbon-based oils, but compatibility must be validated on the finished container because bottle geometry, wall thickness, and mold-in stress influence environmental stress crack resistance more than resin alone. Concentrated nitric acid and strong oxidizing acids are outside the normal service envelope of HDPE. Chlorinated solvents should not be stored at elevated temperatures because solvent permeability and stress cracking can occur. For dangerous goods packaging, the resin itself does not confer UN certification; the finished package must pass the applicable testing under 49 CFR 178 or ADR requirements.
The general technical datasheet for H511W does not by itself certify food-contact compliance under 21 CFR 177.1520; converters requiring food-contact status must obtain written confirmation. The grade is normally specified for non-food packaging where the combination of low melt flow rate, moderate density, and high ESCR is technically relevant.
The processing deviation between H511W and high-flow injection-grade HDPE is not limited to melt flow rate; it affects tool design, cycle time, and part geometry.
| Parameter | H511W | High-flow injection HDPE | Blown film HDPE |
|---|---|---|---|
| Melt flow rate, 190 °C/2.16 kg | 0.30 g/10 min | 5–30 g/10 min | 0.05–0.5 g/10 min |
| Density, ASTM D1505 | 0.951 g/cm³ | 0.950–0.965 g/cm³ | 0.940–0.960 g/cm³ |
| Typical conversion | Extrusion blow molding | Injection molding | Blown film |
| Wall thickness range | 0.5–3.0 mm | 1.0–3.0 mm | 0.02–0.15 mm |
| Primary performance criterion | Parison melt strength and ESCR | Melt flow and cycle time | Tear resistance and film gauge uniformity |
Compared with a general-purpose high-flow injection HDPE, H511W retains a higher melt viscosity at low shear rates, which allows a continuous parison to hold its geometry. Compared with a blown film HDPE at comparable melt index, the density and molecular structure are selected for bottle wall stiffness and low permeability, not for film tear propagation. The addition of post-consumer recycled HDPE can be considered at levels up to 20 wt% if the recycled feedstock is free of polypropylene, polyethylene terephthalate, and paper. If the recycled fraction exceeds 20 wt%, parison sag and melt pressure variability must be validated on the specific blow molder. Published data for H511W-specific recycled-content validation is limited.
For incoming lot acceptance, melt flow rate variation for this material class is typically controlled within ±0.05 g/10 min. When a new lot is received, converters should compare the certificate of analysis against the baseline settings for parison programming and extruder temperature profile. Contamination with other polymer types causes visible delamination or gelling in the finished wall; hopper and conveying systems should be flushed between material changes. The product should be stored in the original sealed containers at temperatures below 50 °C, away from direct sunlight and ultraviolet radiation. Prolonged outdoor storage can reduce the molecular weight of the outer pellet layer and shift melt flow rate readings upward, which would require re-optimization of parison programming.