| HS Code | 610618 |
| Material Type | Polybutylene terephthalate (PBT) |
| Recycled Content | Post-consumer recycled (PCR) grade |
| Filler Content | 15% glass fiber |
| Density | 1.54 g/cm³ |
| Tensile Modulus | 6000 MPa |
| Tensile Strength | 90 MPa |
| Elongation At Break | 2.5% |
| Flexural Modulus | 5500 MPa |
| Flexural Strength | 140 MPa |
| Notched Izod Impact Strength | 5 kJ/m² |
| Heat Deflection Temperature | 200 °C at 1.8 MPa |
| Ul94 Flammability Rating | V-0 |
| Water Absorption | 0.07% |
| Molding Shrinkage | 0.3–0.6% |
As an accredited SABIC VALOX™ PCR PBT T2N815 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | SABIC VALOX™ PCR PBT T2N815 is packaged in 25 kg moisture-barrier bags on pallets for safe storage and transport. |
| Container Loading (20′ FCL) | SABIC VALOX™ PCR PBT T2N815 is palletized and securely loaded into a dry 20-foot FCL container for shipment. |
| Shipping | SABIC VALOX™ PCR PBT T2N815 is shipped as dry, flame-retardant PBT pellets in sealed moisture-barrier bags or boxes. Handle as a non-hazardous solid under normal conditions; keep cool, dry, and away from direct sunlight. Follow local transport and environmental regulations. |
| Storage | Store SABIC VALOX™ PCR PBT T2N815 in a cool, dry, well-ventilated area away from direct sunlight, heat sources, ignition risks, and incompatible chemicals. Keep in sealed original packaging to prevent moisture pickup and contamination. Avoid dust generation and physical damage. Follow the manufacturer’s SDS and local regulations; dry as recommended before processing. |
| Shelf Life | SABIC VALOX™ PCR PBT T2N815 has a typical shelf life of two years when stored unopened in a dry, cool environment. |
Underhood connector housings molded from neat T2N815 for terminal retention features with wall thicknesses from 0.8 mm to 1.2 mm are run on 120-ton to 180-ton hydraulic reciprocating-screw injection machines having L/D ratios of 20:1 to 22:1. The compliance path for 12 V vehicle electrical systems is SAE/USCAR-2 Rev 7, with terminal pull-out, latch deflection, and thermal shock verified after 1,000 h at 125 °C for Class T3 validation. T2N815 is processed at 100 % as-supplied PCR-containing pellet fraction. When in-house runner regrind is used, the regrind addition is capped at 15 % by weight to avoid a measurable shift in melt viscosity and latch creep resistance. Desiccant drying at 120 °C for 4 h is set as the default; if ambient relative humidity exceeds 60 % RH, time is extended to 6 h and dryer dew point is held at or below -40 °C. The barrel profile from feed throat to nozzle is 240 °C, 250 °C, 255 °C, 255 °C, and the mold surface is maintained at 80 °C. Injection velocity is set to 40 mm/s to 60 mm/s with hold pressure 55 MPa to 70 MPa, depending on cavity fill imbalances measured across a 16-cavity family tool. At these settings, production-floor failure is observed as localized gas burn at latch bosses when vent depths exceed 0.02 mm; vents are kept at 0.015 mm to 0.02 mm to prevent flash without trapping volatiles. The terminal product is a multi-pin sealed connector housing with TPA lock, silicone grommet seat, and snap-fit cover, inserted into engine-compartment fuse/relay boxes.
Battery management system wire-to-board connectors operating at 12 V to 48 V cell-sensing potential are molded with T2N815 where the housing must retain creepage distances specified in IEC 60664-1:2020 under pollution degree 2. The terminal product is a modular cell-voltage sense harness header with integral strain relief and board-lock tabs. The PCR mass fraction of the lot is used as supplied, with no virgin dilution, so incoming MFR per ISO 1133-1:2022 at 250 °C / 2.16 kg is treated as the master processing variable. A PBT-based black masterbatch is let down at 2 % to 3 % by weight; a non-PBT carrier at the same let-down ratio is rejected because it shifts the crystallization rate and produces sink marks around the gate land area. The tool is a 2-plate mold with sub-gates of 0.6 mm to 0.8 mm diameter feeding wall sections of 0.5 mm to 1.0 mm. Melt temperature is set at 250 °C, mold temperature at 70 °C, injection speed at 80 mm/s to 120 mm/s for short fill time. Holding pressure is reduced to 45 MPa because excessive packing near fine-pitch partitions causes flash on creepage barriers. The limiting boundary is UL 94 classification: if the pack-level specification requires V-0, T2N815 is not acceptable unless the batch certificate explicitly demonstrates V-0 at the specified wall thickness. For HB-class BMS low-voltage signal paths, the grade is processed with hot-runner valve pin sequencing to avoid dead spots, because an intermittent unmelt at the pin base appears as a brittle partition failure during board insertion. Published data for this specific configuration is limited, so qualification must include 1,000 h at 85 °C/85 % RH per IEC 60068-2-78.
DIN-rail industrial I/O module housings are molded from T2N815 in 8-cavity to 16-cavity valve-gated hot-runner stack tools. The terminal product is an I/O module body with snap-in terminal recesses, ventilation slots, and coding pins, used in control cabinets under IEC 61010-1:2010+A1:2019 and terminal block sub-assembly checks per IEC 60947-7-1:2009. The as-supplied pellet fraction is processed neat to preserve declared recycled content; in-house regrind is not reintroduced in this segment because terminal recess flatness must not drift beyond 0.05 mm after assembly. Drying is executed in a desiccant hopper dryer with inlet air dew point of -50 °C and pellet bed temperature 120 °C for 4 h. Barrel settings are lowered to 245 °C at the nozzle and 240 °C in the compression zone because the hot-runner manifold adds residence time; mold circulation water is set to 60 °C to 70 °C. Due to stack-tool runner volume, hold pressure is set to 60 MPa and back pressure to 0.4 MPa to 0.6 MPa; an MFR shift above 5 % from incoming lot to purged melt indicates hydrolytic degradation caused by wet pellets or hot-runner dead zones. Cavity-to-cavity fill imbalance below 5 % is maintained using manifold thermocouple trim; above that value, terminal recess depth in IEC 60947-7-1 mating acceptance fails on the lower-flow cavities.
Field instrumentation mounting brackets demand post-mold dimensional predictability in a humidity-cycling environment. The terminal product is a transducer housing base with sealing groove, back-shell interference ring, and M12 connector face integrated for IEC 60529 IP67 verification. T2N815 is processed with 1.5 % carbon black masterbatch where UV stabilization is required by the instrument specification; higher loading is not used because the resulting melt viscosity increase reduces fill reproducibility in the sealing groove. The processor dries at 120 °C for 5 h when incoming pellet moisture measured by ISO 15512 exceeds 0.10 %. Mold temperature is set to 90 °C to shift post-mold shrinkage toward the lower side of the ASTM D955 range. After ejection, brackets are annealed at 150 °C for 1 h in a forced-circulation oven; this secondary treatment is introduced because service exposure cycles from -40 °C to 85 °C can otherwise generate warpage at the M12 face. Post-mold shrinkage is measured according to ASTM D955-21 at 24 h and 48 h after molding; unreinforced PBT can exhibit parallel shrinkage values from 0.006 mm/mm to 0.020 mm/mm depending on wall thickness and mold temperature, so grading of T2N815 is lot-specific. Hygroscopic growth is controlled by design: the sealing interface uses a flattened groove bottom with 0.2 mm minimum gasket compression allowance, because unfilled PBT can absorb up to 0.2 % moisture at 23 °C/50 % RH. Published data for this specific configuration is limited; final dimensional capability must be determined from a 3-lot mold qualification.
Power inlet sockets in unattended appliances are positioned below IEC 60335-1:2020 clause 30.2 glow-wire verification. The terminal product is a snap-in appliance power inlet body with earth pin sleeve, shutter carrier, and terminal retention towers, produced from T2N815 when end-product glow-wire requirement is 750 °C for unattended equipment. If the appliance standard or customer specification requires 850 °C ignition resistance with no flame persistence above 2 s, the grade is not automatically accepted; lot-specific glow-wire results under IEC 60695-2-11:2021 must be obtained. The material is treated as 100 % as supplied; no external regrind or additive masterbatch is added because resistance to leakage current across the earth pin sleeve outweighs cost-driven regrind use. Drying follows a desiccant profile of 120 °C for 4 h, but at relative humidity above 70 % RH holding time is extended to 6 h and the hopper is purged with dry air at -50 °C dew point. The tool uses a tab gate of 1.2 mm thickness placed on the non-cosmetic sidewall; melt temperature is set at 255 °C, mold temperature at 90 °C, and hold pressure at 65 MPa to avoid sink over the earth-pin insert. Field data from 80-ton machines shows that insufficient venting of the earth sleeve core produces gas marks visually similar to contamination; the corrective action is core pin venting at 0.015 mm depth and a 3 mm parting-line vent land. The finished socket is subject to IEC 60320-1 dimensional gauging where appl icable; otherwise the end-product appliance standard governs.
LED MR16 lampholder bodies depend on snap-fit retention after insertion cycles at socket temperature. The terminal product is a GU5.3 or GU10 lampholder insulating body with copper contact carriers, strain relief, and lamp-retaining springs. T2N815 is used as the molded insulator when the thermal index under IEC 60838-1:2020 and UL 496 is accepted at the fitted socket temperature. The resin is processed neat, with titanium dioxide added at 1 % only where a white appearance is required; pigmented versions require revalidation of glow-wire and dielectric strength because TiO2 can act as a polar filler and slightly reduce tracking resistance under IEC 60112. Drying is confirmed by moisture analysis below 0.02 %; because the lampholder body has thin snap arms of 0.9 mm to 1.2 mm, a desiccant drying time of 4 h at 120 °C is the minimum. Barrel profile is 245 °C, 250 °C, 250 °C; mold temperature is held at 70 °C; and hold pressure is set at 50 MPa with a short hold time of 3 s to prevent overpacking the snap arms. Weld-line strength is monitored by ISO 527-2 tensile bars cut from the weld area; if weld-line tensile strength falls below 80 % of the non-weld material, gate position is moved to the central pin aperture rather than the rim. Published data for T2N815 in this specific lampholder configuration is limited; qualification must include 500 insertion-extraction cycles under IEC 60838-1:2020 and a dielectric withstand test per IEC 60664-1:2020.
The compliance verification matrix in Table 1 consolidates the application-specific anchors referenced above. No data in the table substitutes for lot-certificate testing.
| Application segment | Primary standard or clause | Critical test condition | Acceptance boundary |
|---|---|---|---|
| Underhood connector housing | SAE/USCAR-2 Rev 7 | 1,000 h heat aging at 125 °C | Terminal pull-out and latch deflection retained after aging |
| BMS signal connector | IEC 60664-1:2020 pollution degree 2 | 12 V to 48 V circuit potential | Creepage/clearance distances per Table F.1/F.2 |
| Industrial I/O module | IEC 61010-1:2010+A1:2019 / IEC 60947-7-1:2009 | Terminal recess flatness post-assembly | Flatness drift ≤ 0.05 mm |
| Field transducer mount | IEC 60529 IP67 | 30 min immersion at 1 m | No ingress at sealing groove and M12 face |
| Appliance power inlet | IEC 60335-1:2020 clause 30.2 | 750 °C or 850 °C glow-wire | No ignition or flame persistence ≤ 2 s where required |
| LED lampholder body | IEC 60838-1:2020 / UL 496 | 500 insertion-extraction cycles | No loss of snap retention or dielectric breakdown |
Table 2 lists starting injection parameters for T2N815 across the same six downstream regimes. These are starting points, not substitute values for mold-specific optimization based on the measured melt flow rate of each batch per ISO 1133-1:2022.
| Application segment | Melt temperature | Mold temperature | Hold pressure | Back pressure | Injection speed |
|---|---|---|---|---|---|
| Underhood connector | 255 °C | 80 °C | 55–70 MPa | 0.5–0.7 MPa | 40–60 mm/s |
| BMS signal connector | 250 °C | 70 °C | 45 MPa | 0.3–0.5 MPa | 80–120 mm/s |
| Industrial I/O module | 245 °C | 60–70 °C | 60 MPa | 0.4–0.6 MPa | 30–50 mm/s |
| Field transducer mount | 250 °C | 90 °C | 50 MPa | 0.5 MPa | 35–55 mm/s |
| Appliance power inlet | 255 °C | 90 °C | 65 MPa | 0.5–0.7 MPa | 40–60 mm/s |
| LED lampholder body | 250 °C | 70 °C | 50 MPa | 0.4–0.6 MPa | 45–65 mm/s |
Competitive SABIC VALOX™ PCR PBT T2N815 prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Material identification for SABIC VALOX™ PCR PBT T2N815 begins with the base polymer, polybutylene terephthalate, a semi-crystalline thermoplastic polyester produced by condensation of 1,4-butanediol with terephthalic acid or dimethyl terephthalate. The ester backbone provides resistance to aliphatic hydrocarbons, alcohols, and many chlorinated solvents; its rapid crystallisation rate contributes to short moulding cycles and high solvent resistance in thin, well-cooled sections. The PCR qualifier in the grade designation indicates that the feedstock includes post-consumer recycled PBT. The recycled fraction is not a separate additive. It is a feedstock stream that can alter molecular weight distribution, carboxyl end-group concentration, nucleation behaviour, and the population of low-molecular-weight volatiles relative to a fully virgin PBT control. Accordingly, the current SABIC technical data sheet and lot-specific certificate of analysis function as the controlling specification documents for exact recycled proportion, melt mass-flow rate, moisture level, and mechanical properties. Published literature for unfilled PBT can be used only as a reference envelope; it cannot replace grade-specific data for T2N815.
Pre-drying is the first boundary condition because polybutylene terephthalate is a condensation polymer that hydrolyses at melt temperature when residual moisture is present. The material should be dried in a desiccant-air dryer with a dew point no higher than -30°C and a drying hopper sized for at least 4 h residence time. A typical drying profile for unfilled PBT is 120°C for 4 h; recycled-containing lots may require 6 h if the pellets have been exposed to ambient humidity above 60%. The target moisture content in the pellets is 0.02% by weight or lower, as measured by ASTM D4019 or ISO 15512. Above that threshold, hydrolysis at melt temperatures over 250°C shortens polymer chains and reduces tensile elongation and notched impact strength. On production-scale dryers, hopper outlet temperature and airflow rate should be recorded because a regenerated desiccant bed that is saturated before the end of the shift will allow moisture breakthrough even if the setpoint display is unchanged.
Drying hopper audits on production lines have shown that a poorly insulated hopper with low purge airflow can leave the pellets 40°C below setpoint while the instrument shows target temperature. The dew-point sensor should be located at the dryer outlet rather than at the regenerated bed inlet. Moisture analysis by a bench-top Karl Fischer coulometer is preferred to loss-on-drying because loss-on-drying can overestimate moisture in recycled PBT due to volatiles other than water. If the material has exceeded the moisture limit, the pellets should not be exposed to temperatures above 140°C for a short quick-dry cycle; prolonged exposure can cause agglomerated pellets and oxidative yellowing.
Barrel temperature profiling on a conventional reciprocating-screw injection-moulding machine normally runs from 240°C at the rear zone to 270°C at the nozzle. The melt temperature should be verified with an immersion pyrometer rather than assumed from setpoints. PBT has a crystalline melting point of approximately 223°C; therefore lower barrel zones below 230°C create solids-bed instability and screw recovery variability. At the upper boundary, thermal degradation accelerates above 270°C. The degradation pathway for PBT can liberate tetrahydrofuran from the butanediol block, which is detectable as an acrid odour at the purge pad and indicates excessive residence time or hot spots. Total residence time from pellet feed to injection should be maintained below 5 min to 8 min. If a machine has a shut-down alarm or a blocked nozzle, the barrel should be purged immediately with a ground PBT regrind or a commercial purging compound free of polyolefin residue. Mixing with polypropylene or polyethylene can create laminate contamination and visible delamination in moulded parts.
Mould surface temperature is critical because PBT crystallises rapidly and the degree of crystallinity affects final part density and shrinkage. A mould temperature between 60°C and 90°C is common for unfilled PBT. If the tool is run at 30°C to 40°C, parts may freeze before complete crystallisation. The result is lower density, higher post-mould shrinkage, and a greater tendency to warp when exposed to elevated service temperature. Cooling circuits should be balanced so that cavity-to-cavity surface temperature variation does not exceed 10°C. Vent depth for PBT should be in the range of 0.012 mm to 0.025 mm; vents are placed at the end of fill and along weld lines. A vacuum-vented tool is sometimes justified for thin-wall connectors because degradation gases and volatile residues from PCR feedstock can deposit on the cavity surface more rapidly than in virgin PBT processing.
Runner balancing on multi-cavity tools should be verified with short shots because a PCR-containing grade may have a slightly different viscosity curve than the virgin material used for initial simulation. Splitter adjustments in cold runners assume Newtonian behaviour; for PBT, the shear-thinning behaviour shifts the balance point, so a geometrically balanced runner is preferred over a family tool with large cavity volume differences. If a hot-runner system is used, the manifold and nozzle temperatures should be independently controlled within a range that prevents freeze-off at the gate but does not expose the material to the upper thermal limit for the duration of the residence time. Gate sizes should be reviewed with the worst-case melt-flow lot in mind. A sub-gate with a sharp transition can create excessive shear heating and gate blush, while a full-round gate in a thick section can cause sink marks if the gate freezes before packing is complete.
Candidate application spaces for SABIC VALOX™ PCR PBT T2N815 include injection-moulded electrical and electronic components such as relay bases, terminal blocks, connector bodies, sensor housings, appliance control brackets, and lighting sockets. The suitability of the material in these applications is conditional on the electrical and thermal parameters of the exact grade. Comparative tracking index, dielectric strength, and UL 94 classification must be taken from the current datasheet and not inferred from PBT family chemistry. In applications where a specific flame class is required, the exact colour and additive package have to be evaluated because recycled feedstock can alter char formation and ignition behaviour. For load-bearing or safety-critical parts, the mechanical property set should be confirmed by testing under ISO 527-2 for tensile properties and ISO 180/1A for notched impact. If those values are not available for the T2N815 datasheet, published data for this specific configuration is limited and a moulding trial is the only valid source of acceptance data.
The melt flow rate of PBT is standardised at 250°C under 2.16 kg using ISO 1133-1:2022 or ASTM D1238. A virgin unfilled PBT grade may be supplied with a narrow melt-volume-flow-rate window; a PCR-containing grade tends to show a wider lot-to-lot range because the post-consumer feedstock includes different molecular weight fractions from different original moulding and extrusion grades. Single-point melt-flow data are insufficient for simulating the fill of thin-wall parts. Capillary rheometry should be performed at apparent shear rates between 102 s-1 and 104 s-1 to obtain the viscosity curve used for gate and runner design. The shear-rate-dependent viscosity is also needed to predict the pressure required to fill a flow-length-to-wall-thickness ratio above 150:1. In these geometries, a lot with a lower melt viscosity will overpack the cavity and create flash, while a lot with higher viscosity will produce short shots or excessive clamp force. Therefore hot-runner or cold-runner tooling for PCR PBT should be designed with adjustable gate sizes or interchangeable tips to accommodate a wider rheological envelope.
Recycled PBT can contain trace particles that promote nucleation. Earlier crystallisation onset reduces effective flow length under identical thermal conditions. On the production floor this is observed as a shorter fill distance before the flow front slows. Moulders sometimes compensate by increasing injection velocity; however, shear heating can raise the melt temperature at the gate and trigger local degradation if the gate is undersized. A gate size of 0.8 mm to 1.5 mm for unfilled thin-wall PBT is a reasonable starting point, but the gate freeze time and shear rate should be confirmed with a short-shot study. Hot-runner tips with internal dead spaces should be avoided because PBT can stagnate and degrade, producing black specks that are more visible in natural or light-coloured PCR-containing parts.
Injection pressure at the nozzle should not be treated as an unlimited lever for recycled PBT. Excessive pressure can overcome viscosity shifts, but it also increases clamp force and can cause jetting, especially in unfilled PBT. A melt-pressure transducer in the nozzle or hot runner provides real-time data to separate machine hydraulic pressure from actual melt pressure. The upper limit is normally dictated by the machine and mould. If a lot requires more than 20% higher melt pressure to fill the same cavity, the lot should be sampled for melt-flow verification before continuing production.
| Property | ASTM method | ISO method |
|---|---|---|
| Melt mass-flow rate | D1238 | 1133-1 |
| Tensile properties | D638-14 | 527-2 |
| Flexural properties | D790 | 178 |
| Notched Izod impact | D256 | 180/1A |
| Heat deflection temperature | D648 | 75-2/B |
| Mould shrinkage | D955 | 294-4 |
| Moisture content | D4019 | 15512 |
| Water absorption | D570 | 62 |
Mould shrinkage for PBT is measured on standard plaques or bars using ISO 294-4 or ASTM D955. Unfilled PBT generally has shrinkage lower than that of semi-crystalline polyolefins, but the exact values depend on wall thickness, flow direction, mould temperature, and holding pressure. A recycled-containing grade can shift the crystallite size distribution and may widen differential shrinkage. For components with snap-fit beams, bearing bores, or insert-moulded terminals, a 24 h post-mould metrology study under controlled temperature and humidity is required. If the part is to be used in an assembly that experiences temperature cycling, dimensional change after 1 h at 120°C or after thermal ageing according to ISO 75-2 should be examined. Published data for this specific configuration is limited; tooling compensation values must be derived from the T2N815 datasheet or from an approved moulding trial, not from a general PBT shrinkage table.
Colour control is a recognised operational limitation for PCR PBT. Post-consumer feedstock can contribute yellow chromophores and occasional microgel specks even after fine melt filtration. If a colour-critical housing or connector is specified, the formulation should be evaluated for CIELAB coordinates under ASTM D2244 with a defined illuminant and observer condition. The recycled fraction may require a higher pigment loading to reach the target chromaticity, which changes melt viscosity and possibly the moulded surface appearance. Spectrophotometric assessment should be performed on a plaque of the production wall thickness, because colour perceived through a thin wall can differ from that of a 3.2 mm test chip. For natural or light-coloured parts, the presence of black specks should be quantified using a defect-count method agreed between moulder and customer. Reducing specks may require finer melt filtration in the compounding step, not simply a higher let-down ratio.
Volatile emissions and odour are additional differences between PCR-containing PBT and virgin PBT. The reclaimed stream can introduce low-molecular-weight oxidation products that are not present at the same concentration in virgin polymer. During moulding, these products may condense on the cavity surface or vent channels. The accumulation is most noticeable on mirror-polished moulds running long production lots. Preventive maintenance intervals for vent cleaning should be shortened when the T2N815 grade is used, and the cleaning agent must be compatible with the mould steel and with the PBT residue. If odour or VOC limits are defined for an automotive interior or appliance application, testing should be performed using the relevant OEM or ISO method. No blanket emission limit should be assumed for the product without a grade-specific test report.
Regulatory compliance for SABIC VALOX™ PCR PBT T2N815 is defined by the manufacturer's product stewardship documentation. RoHS compliance is evaluated against Directive 2011/65/EU and subsequent delegated amendments; the exact grade and colour should be covered by the supplier's declaration. REACH SVHC reporting is required under the current candidate list. If a downgraded risk is needed for a particular market sector, the customer should request a letter from SABIC. The product should not be combined with chlorine- or acid-liberating polymers in a hot-runner system because residual moisture and acids can accelerate polyester degradation. If a food-contact or potable-water application is considered, the exact grade must be covered by an explicit food-contact letter. The presence of PCR feedstock does not automatically exclude the material, but it imposes additional compositional documentation that must be reviewed case by case.
For regrind reuse, PCR PBT does not eliminate the need for closed-loop regrind control. The proportion of regrind should be fixed, and the regrind should be dried under the same dew-point conditions as virgin pellets. Sieve testing of regrind to remove fines below 0.5 mm prevents feeding instability. An increase in regrind content above the allowed percentage alters the melt residence-history distribution and can accelerate yellowing. On a reciprocating-screw machine, feed-throat temperature should remain below 80°C to prevent pellet bridging and premature softening. Caking at the feed throat is more likely if the recycled pellets contain fines or if plant humidity is high.
The main differences between T2N815 and a fully virgin unfilled PBT are expected in the viscosity envelope, colour consistency, melt filtration efficiency, and emission profile. The post-consumer content is qualified by the certification method supplied by the manufacturer and should not be stated as an environmental claim without citing the allocation method. Compared with a glass-fibre-reinforced PBT, the unfilled PCR grade is suitable only for lower-stiffness applications where the flexural modulus of unreinforced polymer is sufficient. Compared with PBT/PET blends, PBT typically crystallises faster and may produce less shrinkage anisotropy, but the exact comparison for T2N815 must be made under the same moulding conditions. Material substitution decisions should therefore be based on a three-part comparison: the technical data sheet values for T2N815, a trial moulding on the intended production tool, and application testing under the relevant ISO or ASTM method.