| HS Code | 187584 |
| Polymertype | Polybutylene terephthalate (PBT), post-consumer recycled (PCR) |
| Reinforcementtype | Glass fiber reinforced |
| Recycledcontent | Contains post-consumer recycled content |
| Flameretardancy | Flame retardant |
| Density | Approx. 1.59 g/cm³ |
| Meltvolumerate | Approx. 15 cm³/10 min at 250 °C/5 kg |
| Tensilemodulus | Approx. 10,000 MPa |
| Tensilestressatbreak | Approx. 130 MPa |
| Elongationatbreak | Approx. 2.0% |
| Flexuralmodulus | Approx. 9,500 MPa |
| Charpynotchedimpactstrength | Approx. 8 kJ/m² at 23 °C |
| Heatdeflectiontemperature | Approx. 200 °C at 1.8 MPa |
| Vicatsofteningtemperature | Approx. 210 °C |
| Ul94flammabilityrating | V-0 |
| Moldshrinkage | Approx. 0.3–0.6% |
| Waterabsorption | Approx. 0.1% at 24 h |
| Processingmethod | Injection molding |
As an accredited SABIC VALOX™ PCR PBT PDR4922 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | SABIC VALOX™ PCR PBT PDR4922 is packaged in 25 kg moisture-resistant bags, palletized and stretch-wrapped for industrial transport. |
| Container Loading (20′ FCL) | SABIC VALOX™ PCR PBT PDR4922 loaded in a clean, dry 20′ FCL container, palletized and secured for safe transport. |
| Shipping | SABIC VALOX™ PCR PBT PDR4922 is supplied as solid polymer pellets in moisture-barrier bags, 25 kg sacks, or octabins. It is generally non-hazardous and not regulated as dangerous goods for transport. Ship in a clean, dry vehicle; protect from moisture, heat, and direct sunlight; follow the SDS and local rules. |
| Storage | Store SABIC VALOX™ PCR PBT PDR4922 in a cool, dry, well-ventilated area, away from direct sunlight, heat, ignition sources, and moisture. Keep containers tightly closed and labeled, protect from dust and physical damage, and avoid humid conditions to prevent moisture uptake. Follow the manufacturer’s SDS and local regulations; use first-in, first-out rotation. |
| Shelf Life | Typically two years from date of manufacture when stored unopened, dry, and cool under SABIC-recommended conditions. |
Underhood sensor housings and camshaft position sensor bodies injection-molded from SABIC VALOX™ PCR PBT PDR4922 require a pre-drying protocol that is stricter than unfilled PBT because the glass reinforcement and the post-consumer recycled polymer fraction both contribute to moisture uptake. The pellets are dried at 120 °C for 4 h in a desiccant-bed hopper dryer supplied with air at a dew point of -40 °C or lower, until residual moisture determined by Karl Fischer titration per ISO 15512 remains below 0.02 wt%. If ambient relative humidity exceeds 60%, the drying time is extended to 6 h and closed-loop material conveying is used to prevent moisture regain before the machine throat. Processing on a reciprocating-screw injection molding machine with an L/D ratio of 20:1 to 22:1 and a compression ratio of 2.0:1 to 2.5:1 is typical; the melt temperature is held at 250 °C to 270 °C, and the mold temperature is maintained at 80 °C to 100 °C to allow sufficient crystallization before ejection. A hot-runner manifold with valve-gated drops is preferred over cold sprue bushings because PBT is sensitive to excessive residence time above 280 °C, which can drive ester bond cleavage and reduce intrinsic viscosity. The glass fiber loading in this grade is specified as 30 wt%; during incoming QC, the ash content should be checked by ISO 3451-1 to confirm batch-to-batch consistency, and the intrinsic viscosity of the PCR PBT fraction should be measured in a 60/40 phenol/tetrachloroethane solvent system at 25 °C per ASTM D4603 to identify lots that have been subjected to hydrolytic degradation during recycling.
For non-safety-critical underhood housings, regrind addition up to 20 wt% is permitted only if the melt flow rate per ISO 1133-1 at 250 °C and 1.2 kg does not shift by more than 15% relative to virgin pellets. The dimensional tolerance on camshaft sensor bodies must be validated across the full thermal shock range mandated by USCAR-2 Class 3 and ISO 16750-4, typically -40 °C to 150 °C for 1000 cycles; a linear mold shrinkage of 0.3% to 0.5% in the flow direction and 0.6% to 0.9% across flow is used as a starting point for tool steel dimensioning. Published data for this specific PCR grade under 85 °C and 85% relative humidity exposure is limited, so tensile retention per ISO 527-2 after 1000 h should be generated for each production lot before qualification for coolant-exposed connectors. Ester bond hydrolysis in SABIC VALOX™ PCR PBT PDR4922 is accelerated by hot ethylene glycol-water coolant mixtures, strong alkalis, and certain amine-based stabilizers. Components located near coolant lines are not recommended unless the OEM specification permits hydrolysis-resistant PBT or the part is externally sealed from continuous liquid contact. Injection operators should avoid purging the barrel with polycarbonate or polyamide without thorough transition cleaning because transesterification or acid-base residues can alter crystallization kinetics. Mold release products containing silicone are acceptable if they do not migrate to the sealing surface; amine-based external release agents are to be excluded.
The charging inlet housing is gated at the thickest section behind the latch boss to produce a balanced fill pattern that minimizes differential glass fiber orientation. Because a 30 wt% glass reinforcement in PDR4922 creates anisotropic shrinkage, the tooling must compensate for a higher across-flow shrinkage than the flow direction; values of 0.3% to 0.5% in the flow direction and 0.7% to 1.0% across flow are used for initial cavity sizing but must be confirmed with a mold-flow simulation using actual PVT data for the PCR lot. Melt temperature is set to 255 °C at the nozzle and 265 °C in the barrel front zone; exceeding 270 °C risks surface splay from degradation gases and increases the probability of black specks from recycled feedstock. Injection speed is profiled from 40 mm/s at the gate to 120 mm/s during the filling phase, with a switch-over at 95% of stroke by volume and a holding pressure of 60 MPa to 80 MPa for 8 s to 12 s. The mold temperature is maintained at 90 °C because higher mold temperatures reduce frozen-in orientation and lower the post-mold warpage after thermal cycling per IEC 62196-1.
The material does not carry an inherent V-0 UL 94 rating; when the charging inlet is classified as a live part or is subjected to a 650 °C glow-wire test under IEC 60695-2-11, an approved flame-retardant grade or a co-molded shield is required. For non-current-carrying brackets, latch carriers, and cable strain-relief housings, UL 94 HB is acceptable if the application standard does not require a higher class. Dimensional stability must be verified after 48 h at 90 °C and 95% relative humidity; a change in critical latch span exceeding 0.15 mm is cause for gate relocation or holding-pressure re-optimization. The PCR fraction in PDR4922 can widen the melt viscosity distribution compared with a virgin PBT of the same glass loading, so molders should log screw recovery time and melt cushion variation for each shot. A melt cushion change greater than 2 mm within a production run indicates inconsistent feedstock or moisture ingress, both of which will alter charging inlet latch retention force after conditioning.
Because multi-cavity relay base tooling exposes the melt to longer residence times than single-cavity automotive sensor tools, the screw rotation speed should be limited to 80 rpm and the back pressure to 0.5 MPa to 1.0 MPa to avoid excessive shear heating. The melt temperature for SABIC VALOX™ PCR PBT PDR4922 is held at 250 °C to 260 °C, and the mold temperature is set at 70 °C to 80 °C for acceptable cycle time without sacrificing crystallization. Brass terminal inserts are preheated to 120 °C in an induction or hot-air station immediately before placement; cold inserts draw heat from the PBT melt and can produce a brittle crystalline rim at the insert interface. Regrind addition up to 30 wt% is permitted for relay bases if the melt flow rate per ISO 1133-1 at 250 °C and 1.2 kg remains within 10% of the virgin lot and the regrind is dried to 0.02 wt% moisture. Electrical safety is evaluated by IEC 60664-1 for creepage and clearance dimensions and UL 94 HB for flammability; the comparative tracking index measured per IEC 60112 is used to set minimum creepage distance. A relay base molded in glass-reinforced PBT typically requires a minimum wall thickness of 1.5 mm around live metal inserts, but the exact creepage requirement shall be calculated from the working voltage and pollution degree specified by the end-use standard. Terminal retention force after 500 h at 125 °C is measured by push-out testing per the OEM drawing; a loss exceeding 20% of initial retention indicates insufficient insert preheat or excessive molded-in stress.
| Application sector | Primary test standard | Test condition | Controlled parameter |
|---|---|---|---|
| Underhood sensor housings | USCAR-2 Class 3 / ISO 16750-4 | -40 °C to 150 °C, 1000 thermal cycles | Dimensional change, contact integrity |
| EV charging inlet housings | IEC 62196-1 / IEC 60695-2-11 | 650 °C glow wire, 90 °C / 95% RH, 48 h | Latch span change, ignition persistence |
| Industrial relay bases | IEC 60664-1 / IEC 60112 | Pollution degree 2, working voltage per end-use | Creepage distance, CTI |
| Power tool gearcases | IEC 60745-1 / ISO 179-1/1eA | -20 °C drop impact, notched Charpy | Crack initiation, impact energy |
| LED driver enclosures | UL 8750 / UL 746B / IEC 60695-10-2 | 125 °C ball pressure, RTI aging | Softening, long-term thermal retention |
| PV DC connector bodies | IEC 62852 / ASTM G154 | 85 °C / 85% RH, 1000 h; UV cycle 1 | Wet insulation resistance, surface embrittlement |
A 30 wt% glass fiber loading in SABIC VALOX™ PCR PBT PDR4922 reduces linear mold shrinkage to 0.3% to 0.5% in the flow direction, which helps maintain bearing bore concentricity in gearcase halves, but it also raises the melt viscosity enough to require a high-pressure injection system. The mold is designed with a sprue diameter of at least 3.0 mm and full-round runners 5.0 mm to 6.0 mm in diameter to minimize shear heating. The cylinder temperature profile is set from 240 °C at the rear zone to 265 °C at the nozzle, and the mold temperature is maintained at 80 °C to 90 °C. For gearcases that must pass a drop impact test at -20 °C per IEC 60745-1, the notched Charpy impact strength measured on dry-as-molded specimens per ISO 179-1/1eA is a more reliable incoming QC gate than tensile strength alone; a typical acceptance window for 30 wt% glass-reinforced PBT is 6 kJ/m² to 9 kJ/m², but published data for this specific PCR configuration is limited, so the threshold must be established against an approved virgin PBT control. Regrind levels above 20 wt% shift the melt flow rate and increase the risk of fiber breakage during recompounding, which lowers tensile strength at break per ISO 527-2 and can cause bearing bosses to crack after 500 h of vibration testing.
The operator should monitor screw recovery time and plasticating pressure; a change of more than 10% between virgin and 25 wt% regrind indicates that the regrind is generating excessive fines. Gas-assisted injection molding is used for thick-walled gearcase sections to prevent sink marks, with gas pressure at 20 MPa to 30 MPa and a gas delay time of 1 s to 2 s after melt injection. The use of an amine-free antioxidant masterbatch at 0.2 wt% may be considered for extended thermal stability, but it must be pre-compounded and not tumble-mixed to avoid localized degradation. Motor brush cards and trigger housings molded from PDR4922 must be checked for weld-line strength because multi-gated tools create knit lines at high glass orientation boundaries; the weld-line tensile strength per ISO 527-2 is typically 30% to 50% lower than the bulk value and must be accounted for in rib and boss placement.
Thin-wall sections below 1.2 mm in LED driver enclosures require a melt temperature at 270 °C and a mold temperature of 100 °C to prevent premature freeze-off and to promote sufficient crystallization for dimensional stability. The high mold temperature increases cycle time but reduces post-mold shrinkage in the 0.8 mm to 1.5 mm wall-thickness range that is common for driver housings. SABIC VALOX™ PCR PBT PDR4922 is not inherently UV-stabilized; if the enclosure is visible through a luminaire aperture, an ultraviolet absorber package is required, and the compounded part must be tested per UL 746C outdoor suitability protocols. Continuous service temperature is determined by the relative thermal index listed in the UL 746B yellow card for the exact color and wall thickness; for glass-reinforced PBT grades, RTI values are typically between 120 °C and 140 °C, but the PCR lot must not be assumed to inherit the virgin grade RTI without supplementary long-term thermal aging data. Ball-pressure relief at 125 °C per IEC 60695-10-2 is evaluated on the final molded part because the glass fiber orientation near the gate can create a localized anisotropic softening response.
In photovoltaic junction box and cable gland applications, the molded surface of SABIC VALOX™ PCR PBT PDR4922 is subjected to simultaneous UV irradiance, thermal cycling, and damp heat, which places different demands on the polymer than indoor industrial components. Molding is conducted with a melt temperature of 255 °C and a mold temperature of 90 °C; the tool is generally hot-runner with a balanced manifold and small gate vestiges to reduce mechanical stress on thin snap-fit features. A carbon black or UV-stabilized masterbatch is added at 2 wt% to 4 wt% by weight if outdoor exposure is specified, because unfilled and glass-reinforced PBT without UV protection embrittles rapidly under ASTM G154 cycle 1 exposure. Compliance for photovoltaic connectors is controlled by IEC 62852, which includes damp heat at 85 °C and 85% relative humidity for 1000 h, thermal cycling from -40 °C to 85 °C, and wet insulation resistance testing. The use of PDR4922 in live contact carriers requires a creepage distance calculated according to the pollution degree and comparative tracking index measured per IEC 60112; if the CTI of a particular PCR lot falls below 250 V, the design must be revised or the material rejected for that component. Avoid contact with strong alkaline cleaning agents used in solar farm maintenance, as PBT is susceptible to stress cracking under load in alkaline environments; cleaning validation should follow ASTM D543 with the specific cleaning concentrate and a 0.5% externally applied strain.
Competitive SABIC VALOX™ PCR PBT PDR4922 prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
SABIC VALOX™ PCR PBT PDR4922 is a semi-crystalline polybutylene terephthalate injection-molding resin containing post-consumer recycled feedstock. The grade belongs to the VALOX PCR series and is supplied as compounded pellets for conventional reciprocating-screw injection molding of electrical, automotive, and industrial components. Because PBT crystallizes rapidly, the effective process window is narrower than that of amorphous polycarbonate or some polyamide grades, and mold temperature control is a primary determinant of part quality. The following technical profile identifies processing constraints, batch-to-batch variation, and substitution limits relevant to PDR4922. Grade-specific mechanical specifications must be read from the current SABIC datasheet and lot certificate of analysis.
Recycled-content allocation for SABIC circular grades is site-specific. PDR4922 may be supplied under a mass-balance or segregated post-consumer recycled stream; the designation does not by itself state a fixed percentage. Users preparing environmental claims should obtain lot-level certification under ISCC PLUS or equivalent and review the claim against ISO 14021 self-declared environmental claims. The grade is commonly supplied in black or dark tones depending on the PCR stream, which can influence laser marking, color consistency, and aesthetic acceptance.
Hydrolytic chain scission is the dominant degradation mechanism. PBT contains ester groups that cleave in the presence of residual moisture above 0.02% by weight at melt temperatures. Pre-drying in a desiccant dryer at 120 °C for 4 h is the class-typical starting point; supply air dew point should remain between -30 °C and -40 °C. Hopper dryers without desiccant beds are unsuitable when ambient relative humidity exceeds 60% because they cannot maintain the required moisture endpoint. Residual water causes molecular weight reduction, viscosity loss, reduced tensile elongation at break, and increased gate-splay defects.
| Parameter | Setpoint | Reference / note |
|---|---|---|
| Drying temperature | 120 °C | Desiccant dryer |
| Drying time | 4 h | Newly opened bulk containers |
| Maximum residual moisture | <0.02% | ISO 15512 or equivalent |
| Dew point | -30 °C to -40 °C | Dryer supply air |
| Melt temperature | 245 °C to 260 °C | Unfilled PBT class |
| Mold temperature | 60 °C to 90 °C | For crystalline development |
| Maximum residence time | ≤5 min | Below melt upper limit |
The table above lists class-typical injection-molding parameters for unfilled PBT. Grade-specific PDR4922 values should be taken from the supplier datasheet because post-consumer fractions can shift the melt volume-flow rate relative to virgin PBT with the same nominal viscosity. Melt temperature selection is also constrained by the upper limit of 270 °C; above this, terephthalate degradation produces volatile condensates that plate out on mold surfaces and vent channels. Nozzle temperature should be maintained at 250 °C to 260 °C for short nozzles, but reduced to 245 °C if the nozzle body is long or externally heated band control is unstable.
Recycled PBT may exhibit a wider molecular-weight distribution than virgin PBT, so exact melt residence time must be controlled. At a melt temperature of 245 °C to 260 °C, maximum barrel residence time should not exceed 5 min. Prolonged residence time in hot runners or oversized barrels accelerates darkening, acetaldehyde evolution, and additional chain scission. On production-scale machines with barrel L/D ratios above 20:1, the dosage stroke should be set so that shot mass remains within 30% to 70% of barrel capacity to minimize recirculated melt. If a machine is stopped, the barrel should be purged with a non-hygroscopic purge compound before shutdown.
Rheological response during filling is shear-thinning; the grade exhibits typical unfilled PBT flow behavior rather than the highly pseudoplastic response of glass-filled compounds. When gate velocity is too low, the melt freezes before packing, causing underpacked parts and high shrinkage variation. Medium-to-fast injection speeds with a moderate hold pressure profile reduce sink marks in thick sections. Screw back pressure in the range 30 bar to 70 bar and screw surface speed below 0.3 m/s are typical for unfilled PBT; exact values must be adjusted to lot-specific melt volume-flow rate measured under ISO 1133-1:2022 at 250 °C and 2.16 kg.
Hydrolysis is autocatalytic once free carboxylic acid end groups form; molecular weight loss accelerates. Drying to below 0.02% moisture is insufficient if pellets are exposed to humid air before entering the feed throat. Moisture regain can occur within minutes in an open hopper at 60% relative humidity. A closed, heated hopper or direct vacuum loader is therefore required in high-humidity production environments. Screw design should use general-purpose polyolefin geometry with L/D 18:1 to 22:1 and compression ratio 2.4:1 to 3.0:1. High-shear mixing sections are not required for unfilled PBT and can generate excessive melt temperature, especially when PCR feedstock contains trace polyolefin contamination.
Unfilled PBT crystallizes rapidly, and mold temperature determines the degree of post-mold crystallization. Mold temperatures of 60 °C to 90 °C are required to stabilize mold shrinkage and reduce warpage. For unfilled PBT compositions, mold shrinkage parallel to flow is commonly reported in the 1.5% to 2.0% range, with transverse shrinkage slightly lower. However, published data for this specific configuration is limited; recycled-stream variability can shift shrinkage by a measurable amount. Dimensional capability studies on an existing production tool should therefore use lot-representative PDR4922 material, not virgin PBT reference data.
Post-mold crystallization continues after ejection. If parts are measured immediately, dimensions may drift until equilibrium crystallinity is reached. A conditioning period at 23 °C and 50% relative humidity for at least 24 h is required before metrology in accordance with ISO 291. Post-consumer PBT may contain trace PE, PP, or PET fractions that alter nucleation density and crystalline morphology. These contaminants can produce local shrinkage heterogeneity, visible as flow lines or non-uniform gloss. Melt filtration by the compounder reduces but does not eliminate particulate contamination; critical sealing and snap-fit features require process validation.
Venting depth for unfilled PBT is typically 0.015 mm to 0.025 mm for the first 3 mm to 5 mm of land length. Recycled grades may require widened vents or more frequent cleaning due to oligomer deposition. Inadequate venting leads to burn marks at the end of fill and reduced weld-line strength. Hot runner systems should use internally or externally heated manifolds with small melt channels. Melt residence volume in the hot runner should be less than one shot volume to avoid dead spots. If the hot runner contains unmixed PCR fractions, black specks or gloss variation may appear. A shutoff nozzle is preferred over an open nozzle to prevent drooling during screw recovery.
Regrind from sprues and runners can be re-melted but must be ground, stored dry, and re-dried. Because PCR feedstock already has a thermal history, adding more than 20% regrind may push the cumulative heat exposure beyond acceptable limits for notched impact and color consistency. If the application requires tight impact retention, regrind use should be excluded or validated at the final wall thickness. For tight dimensional targets, mold temperature variation across the cavity should be held within ±5 °C to avoid differential crystallization and warpage.
Direct substitution on a tool qualified with virgin VALOX 310 or 325 is not a material-number change; it is a process revalidation. The first comparison should be melt volume-flow rate under ISO 1133-1:2022 at 250 °C and 2.16 kg. If the PDR4922 melt volume-flow rate differs from the incumbent by more than ±15%, filling pressure, gate freeze time, and packing pressure must be recalculated. Thin-wall parts below 1.0 mm nominal wall thickness are more sensitive to melt-flow shifts than thick-wall parts.
Mechanical allowables should be re-established using ISO 527-2 tensile stress and elongation, ISO 178 flexural modulus, and ISO 180/A notched Izod impact. Because recycled PBT streams may contain degraded polyesters, notched impact and tensile elongation at break are more likely to fall below virgin PBT values even when tensile strength remains comparable. Parts with living hinges, snap fits, or cold-impact requirements should be tested at the lowest service temperature, typically -30 °C for automotive interior clips, rather than at ambient laboratory conditions.
Color and odor constraints differ from neat polymer. Post-consumer recycled PBT is commonly supplied in black or dark tones, which restricts color-matching capability compared to virgin natural grades. Residual volatile compounds from prior use may increase mold deposit formation in the venting areas. Tool maintenance intervals may decrease when running PCR feedstock; vent plugging and cavity staining are typically observed on production-scale machines after prolonged runs. If the application is odor-sensitive or requires a light color, a segregated natural PCR stream or a different grade should be selected.
PDR4922 remains an unfilled PBT; it is not a direct replacement for glass-fiber-reinforced VALOX grades such as 420SEO. A 30% glass-reinforced PBT can exhibit flexural modulus above 7000 MPa under ISO 178, while unfilled PBT typically remains near 2500 MPa. The recycled grade should therefore not be used in structural housings or brackets designed around glass-filled stiffness. Similarly, if a UL 94 V-0 rating is required in the existing application, PDR4922 must be tested in the final wall thickness and color; the PCR grade is not automatically assigned the same flammability rating as flame-retardant VALOX compounds. Electrical property requirements such as comparative tracking index under IEC 60112 or volume resistivity under IEC 62631-3-1 require end-part evaluation because PCR contaminants can affect surface resistivity.
Operational boundaries include avoiding combination with amine-based additives or flame retardants that may accelerate polyester chain scission. Drying above 130 °C for extended periods should also be avoided because oxidative yellowing can occur. Aggressive hot-runner residence time above 5 min is not recommended. Un-dried regrind should not be blended into PDR4922 unless the regrind has been re-dried to below 0.02% moisture. Regrind addition should be limited to the same grade and kept below 20% in applications with demanding mechanical or electrical requirements unless lot-specific validation shows otherwise.
| Item | Standard / regulation | Typical required evidence |
|---|---|---|
| Density | ISO 1183-1 | Lot certificate |
| Melt volume-flow rate | ISO 1133-1:2022 | Lot certificate |
| Tensile stress at yield | ISO 527-2 | Lot certificate |
| Notched Izod impact | ISO 180/A | Lot certificate |
| Heat deflection temperature | ISO 75-2/Ae | Lot certificate |
| Recycled-content claim | ISO 14021 | ISCC PLUS or equivalent certification |
| Moisture content | ISO 15512 | In-house check before molding |
| Flammability rating | UL 94 | Grade-specific UL card |
Lot-specific certificates of analysis should be reviewed before each production order because post-consumer feedstock composition varies by source. A processing adjustment made for one lot may not transfer to the next without revalidation. Grade-specific values for density, melt volume-flow rate, tensile stress, flexural modulus, notched Izod impact, and heat deflection temperature must be taken from the current SABIC datasheet for VALOX PCR PBT PDR4922 rather than from generic PBT family data.