| HS Code | 411577 |
| Polymer Type | PBT with 30% glass fiber reinforcement and hydrolytic stabilization |
| Mold Shrinkage Flow Percent | 0.2-0.5 |
| Ul94 Flame Rating | V-0 at 0.8 mm |
| Volume Resistivity Ohm Cm | 1E15 |
As an accredited SABIC VALOX™ PBT+GF30%-Hydrolytic K4560 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | SABIC VALOX™ PBT+GF30%-Hydrolytic K4560 is supplied in 25 kg moisture-resistant bags, palletized for industrial handling. |
| Container Loading (20′ FCL) | 20′ FCL loading: SABIC VALOX™ PBT+GF30%-Hydrolytic K4560 in palletized 25 kg bags, shrink-wrapped, secured, and evenly distributed for ocean transport. |
| Shipping | SABIC VALOX™ PBT+GF30%-Hydrolytic K4560 is shipped as non-hazardous thermoplastic pellets in moisture-barrier bags within sealed drums, octabins, or bags. It is not regulated for transport under UN/DOT/IMDG/IATA. Keep dry, avoid heat, moisture, and contamination; store in original sealed packaging. Handle carefully to prevent package damage. |
| Storage | Store SABIC VALOX™ PBT+GF30%-Hydrolytic K4560 in a cool, dry, well-ventilated area, away from direct sunlight, heat, and moisture. Keep in sealed original packaging to prevent humidity uptake. Maintain stable stacking, avoid incompatible chemicals, and follow the SDS and local regulations. |
| Shelf Life | SABIC VALOX K4560 has a typical shelf life of two years under dry, cool, unopened storage conditions, protected from moisture and sunlight. |
Specification of a 30 wt% glass-fibre-reinforced, hydrolytically stabilised polybutylene terephthalate for under-hood electrical connectors is driven by the requirement that hydrolytic chain scission at the carboxylic ester repeat unit does not reduce tensile elongation below harness retention thresholds in hot ethylene glycol–water mixtures and humid under-bonnet air. In this application, K4560 is introduced as the insulation-carrier resin at 100 parts by weight of the injection-moulding compound; any colour concentrate is pre-dispersed in a polyester carrier and added at 0.8–1.2 wt% relative to total shot mass, while post-industrial regrind from sprues, runners and rejected mouldings is capped at 20 wt% because cumulative shear history lowers molecular mass and accelerates surface crack initiation at glass-fibre ends. Compliance is normally structured around USCAR-2 performance class 3, ISO 16750-4 damp heat 85°C/85% RH, and ISO 6722 for adjacent cable-harness compatibility. Moulding is performed on a closed-loop electric injection moulding machine with a screw L/D ratio of 20:1 to 22:1, compression ratio 2.0:1 to 2.5:1, melt temperature 250°C to 265°C at the nozzle, mould temperature 80°C to 95°C, holding pressure 60–80 MPa, and gate diameter not less than 0.8 mm for 2.0 mm wall sections. Terminal finished product types include engine-control-unit connectors, transmission harness connectors, front bulkhead junction-box covers, and under-bonnet sensor interfaces. Processing above 270°C or residual moisture above 0.02 wt% prior to plasticising negates the stabilisation package by elevating carboxylic-acid end-group concentration beyond the design envelope.
In washing-machine circulation pumps and dishwasher heat-exchanger manifolds, K4560 is processed into impellers and volutes at a melt temperature of 250°C to 265°C and a mould temperature of 80°C to 100°C; low mould temperature below 60°C produces frozen-in orientation at glass-fibre ends and creates microchannels that detergent surfactants penetrate. The resin is fed at 100 parts by weight as supplied, with 1.5–2.0 wt% of a carbon-black/antioxidant masterbatch when UV-stable black parts are required; no additional glass fibre or impact modifier is specified because the 30 wt% glass reinforcement already controls creep under pump head pressure up to 0.4 MPa. Industry compliance is evaluated under IEC 60335-1 and IEC 60335-2-5/IEC 60335-2-7 with 10-day water-immersion ageing at 80°C in a 0.15% sodium C12 alkyl sulphate solution; hydrolytic stability is accepted by retained tensile strength at break according to ISO 527-2:2012 and by visual inspection for surface blistering after ageing. The production process is injection moulding with a sequential valve-gated hot-runner system, screw back-pressure 5–8 MPa, injection velocity 60–100 mm/s, and decompression stroke not exceeding 3 mm to avoid air entrapment. Field failure data from service pumps indicate that hydrolysate-induced fibre whitening appears at the weld line on the impeller hub before loss of pressure; this is delayed by increasing mould temperature to 90°C and reducing residence time to below 240 seconds. Terminal finished product types include washing-machine drain-pump casings, dishwasher circulation-pump volutes, and heat-exchanger end caps.
Municipal water distribution and building services specify 30 wt% glass-reinforced hydrolytically stabilised PBT where brass dezincification and polyphenylene sulfide crystallinity create cost or stress-cracking issues in water-contact components. K4560 is used at 100 parts by weight; for potable-water contact, the only permitted concentrate is a 1.0–2.0 wt% phthalocyanine-free blue or carbon-black masterbatch that carries NSF/ANSI/CAN 61 certification for the specific colourant and final formulation. Compliance for the material is established through NSF/ANSI/CAN 61, AS/NZS 4020, and ISO 4064 for metrological endurance testing; for internal pressure-bearing components, EN 1567 and EN 12201 apply only after verifying the creep rupture envelope at the moulded thread-boss geometry. Processing on a two-stage injection-moulding machine with a screw diameter of 40 mm to 60 mm and L/D 20:1, melt temperature 250°C to 260°C, mould temperature 70°C to 90°C, and holding pressure 70–90 MPa yields a leak-tight amorphous skin; cooling time scales with wall thickness squared divided by thermal diffusivity, typically 12–18 s for a 4 mm body wall. Terminal finished product types include cold-water and hot-water valve bodies rated to 80°C intermittent service, water-meter piston carriers, and municipal backflow-preventer sleeves. Published data for K4560 in potable-water immersion beyond 12 months is limited; qualification must be based on component-level accelerated extraction testing and periodic in-service audit.
Although photovoltaic enclosures do not see continuous liquid water, diurnal temperature cycling creates internal condensation, and the junction-box body must retain impact resistance and screw-boss torque after 25-year damp-heat excursions. K4560 is processed with 100 parts by weight of as-supplied compound; no regrind is permitted in components intended for UL 746C outdoor-use recognition unless the regrind ratio is below 10 wt% and each lot is dried to 0.02 wt% or less by Karl Fischer titration. Compliance is verified under UL 746C for outdoor suitability, IEC 61215-1:2021 damp-heat 85°C/85% RH for 1000 h, and the appropriate photovoltaic connector standard such as UL 373 where terminal retention is assessed; flame class must be confirmed separately because hydrolytically stabilised PBT GF30 is not inherently V-0. Production uses a moulded-part insert-and-overmould process on a vertical injection machine with clamp force of 120–180 t, melt temperature 255°C to 265°C, mould temperature 80°C, and hot-runner drop diameter from 2.5 mm to 4.0 mm; seal-interface flatness is held below 0.15 mm across a 150 mm diagonal by adjusting the holding-pressure profile. Terminal finished product types include photovoltaic junction-box lower housings, DC connector shells, and microinverter terminal covers. Field observation connects screw-boss cracking after 2000 h damp heat to glass-fibre orientation convergence at the boss root; redesign of boss diameter to 2.5 times the screw nominal diameter and mould temperature of 85°C reduces failure frequency.
Sectioned busbar insulators in industrial switchgear and motor control centres require high arc resistance, low moisture-induced dimensional change, and sufficient stiffness to support copper busbar under short-circuit magnetic forces. The formulation for busbar insulators uses K4560 at 100 parts by weight; addition of 0.5 wt% air-release masterbatch is permissible, but mineral filler addition above 3 wt% is not advised because reduction of effective glass content below 30 wt% undermines flexural modulus at elevated temperature; higher flame retardance must be re-qualified with a flame-retardant PBT grade rather than dry-mixing FR masterbatch. Compliance is tested to IEC 60664-1 for creepage and clearance, ASTM D3638 comparative tracking index, and ISO 527-2 for flexural modulus; electrical property retention is normally measured after 85°C/85% RH ageing for 500 h. The production route is injection moulding with decompression setting 3–5 mm, cushion 3–5 mm, melt temperature 250°C to 265°C, and mould temperature 75°C to 90°C; long glass-fibre distribution through a 4 mm wall creates a three-layer shell-core orientation morphology that produces differential shrinkage of 0.25% in the flow direction and 0.70% transverse, so mould design must allow asymmetric core pins and venting along the weld line. Terminal finished product types include multi-pole busbar insulators, terminal-block bases, and switch-disconnector insulating supports. Field failure records show that hot spots above 110°C at copper–PBT interfaces induce local hydrolysis and must be controlled by limiting current density at the interface to below 1.5 A/mm².
K4560 is moulded into condensate-pump motor end-covers for condensing boilers and HVAC condensate-removal modules, where the part is exposed to condensed flue-gas condensate with pH 3.0–4.5 and tray temperatures up to 70°C. The formulation ratio is 100 parts by weight K4560; 1.0 wt% acid-scavenger masterbatch may be added for low-pH condensate aggressiveness, but addition above 1.5 wt% reduces melt fluidity and produces screw slippage in the plastication unit. Compliance is anchored to EN 60335-1, IEC 60335-2-40, and the UL 94 classification listed on the supplier datasheet; severe acid-condensate exposure is evaluated by immersion in pH 3.5 sulfuric/acetic acid solution for 1000 h. The injection-moulding process requires pre-drying at 120°C for 4 h with dew point below −30°C, melt temperature 250°C to 260°C, mould temperature 80°C, and a screw with effective L/D of 20:1; the end-cover boss is moulded with a collapsible core to avoid post-mould drilling that exposes unskinned glass-fibre ends to condensate. Terminal finished product types include condensate-pump end-covers, boiler flue-collector internal brackets, and heat-pump reversing-valve coil insulators. Published data for K4560 under pH 3.5 condensate ageing is limited; process validation should include dimensional change measurement and leak-tightness after 1000 h exposure.
Competitive SABIC VALOX™ PBT+GF30%-Hydrolytic K4560 prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
SABIC VALOX™ K4560 is a hydrolytically stabilised polybutylene terephthalate compound containing 30% glass-fibre reinforcement. The grade is intended for injection-moulded components that must retain dimensional, mechanical, and electrical-insulation performance after exposure to hot aqueous media, engine coolant mixtures, or condensing humidity. Published typical values for density are approximately 1.53 g/cm³ per ISO 1183-1; mould shrinkage is typically 0.2–0.4% in the flow direction and 0.5–0.8% transverse to flow when measured according to ISO 294-4. The hydrolysis-stabilised chemistry differentiates it from standard PBT/GF30 grades, in which ester linkages undergo progressive chain scission in hot water or glycol solutions. Applications include underhood connector bodies, sensor carriers, relay housings, and pump housings where cyclic exposure temperature remains within the continuous-use limit of the design. Selection for production should be validated using ISO 16750-4 thermal/humidity profiles, USCAR-2 connector qualification, or an equivalent OEM specification; public quantitative data for K4560 in every fluid-exposure combination is limited.
Under hot-fluid exposure, unmodified PBT hydrolyzes through autocatalytic chain scission because the acid end groups generated during ester cleavage accelerate further degradation. In a 50/50 water/ethylene glycol mixture at 125°C, standard PBT/GF30 often loses tensile strength at weld lines, gate regions, and sharp radii before bulk material failure. A hydrolytically stabilised grade retards this ester hydrolysis and may shift the limiting failure mechanism toward interfacial effects: fibre/matrix debonding, capillary wicking along glass bundles, and conductive deposit formation on connector pins. Qualification studies should therefore measure insulation resistance after condensation cycling and dimensional change after thermal shock rather than relying solely on tensile retention.
Hydrolytic stabilisers function as an acid-scavenging or end-capping system in the polymer matrix; they do not prevent steam hydrolysis of wet pellets inside the barrel. In melt-phase processing with residual moisture above 0.02%, polymer degradation occurs too rapidly for the stabiliser to compensate. Published data for K4560 in 50/50 coolant at 125°C should be obtained from SABIC or evaluated on moulded plaques because retention depends on glass sizing, weld-line placement, and part thickness.
From a kinetic standpoint, solid-state hydrolytic degradation of PBT is strongly dependent on water concentration, temperature, and part thickness. Thin-wall sections equilibrate more quickly with humid surroundings but dry faster; thick sections can retain water near the glass-fibre interface and continue hydrolysis after the external environment returns to ambient conditions. Design reviews should therefore map cooling-circuit proximity to maintain mould temperatures within the recommended range and reduce internal stress concentrations that accelerate environmental stress cracking at glass-fibre ends. Compared with hydrolysis-resistant PBT/PET blends, K4560 retains the faster crystallisation behaviour of PBT, which supports shorter cycle times and easier ejection, but the maximum continuous-use temperature in hot coolant must still be limited by hydrolysis kinetics rather than by dry heat-deflection temperature alone.
Because glass-fibre reinforced PBT shrinks anisotropically, tool compensation must account for flow-direction shrinkage of 0.2–0.4% and transverse shrinkage of 0.5–0.8% rather than using an isotropic average. In a multicavity connector tool, cavity-to-cavity dimensional variation is driven by differences in fill speed, holding-pressure transmission, gate-seal time, and fibre orientation. A 20 mm aperture can differ by 0.08–0.16 mm between flow and cross-flow directions if the tool is not corrected.
Production-scale injection moulding on 80–120 t clamp force machines with 20:1 L/D general-purpose reciprocating screws is typical; the holding-pressure profile should be set using cavity-pressure transducers positioned at the last-filling area and near the gate. Conventional hydraulic injection pressure for thin-wall PBT/GF30 connectors usually falls between 80–120 MPa, while mould-temperature-control units using pressurised water at 80–95°C improve crystallinity and reduce moulded-in stress but increase cycle time and may require oil circuits if water pressure limits are exceeded.
Weld lines in glass-filled PBT are weak because fibres align parallel to the weld interface rather than crossing it. Local tensile strength at a weld line may be 30–50% lower than the bulk value. For coolant-exposed parts, a weld line placed in a seal groove or snap-fit root can become a preferential pathway for fluid ingress and subsequent hydrolysis, even when the bulk material passes accelerated aging tests.
Post-mould annealing at 120–140°C for 2–4 h can reduce internal stress and increase crystallinity, but it also increases shrinkage and can degrade the hydrolytic stabiliser if the temperature exceeds formulation limits. Annealing trials should be run on parts with critical dimensions measured before and after treatment to separate reversible dimensional changes from permanent tool-adjustment needs. This is especially important for parts that will be assembled with press-fit contacts, where post-annealing growth can change insertion force.
Before moulding K4560, the pellets must be dried to residual moisture below 0.02%. A desiccant-bed dryer set at 120°C with a dew point of -40°C or lower and a residence time of 3–4 h is standard. Overdrying beyond 6 h at 140°C should be avoided because oxidative yellowing can occur before melt processing. Barrel temperatures from feed to nozzle are typically 240°C, 250°C, 260°C, and 260°C; melt temperature measured by an insertion thermocouple should remain between 250°C and 270°C. Mould temperature should be controlled at 65–95°C, with the upper end improving crystallinity but extending cooling time.
Back pressure of 3–7 bar hydraulic and screw surface speed of 0.2–0.4 m/s help preserve glass-fibre length during plastication. Shot size should be 30–70% of barrel capacity, and total residence time in the barrel should not exceed 8 min at melt temperature. Vented barrels are not recommended because hydrolysis of glass sizing or polymer during devolatilisation can offset the stabiliser effect. Lot-to-lot incoming inspection should record ash content per ISO 3451-1 and melt volume-flow rate per ISO 1133-1:2022 to detect glass-fibre content or molecular-weight deviations before moulding begins. If the machine has a hot runner, the manifold and nozzle tips should be heated with independent zones and shielded from prolonged residence time. Dead spots in hot-runner drops can create black specks and acid-catalysed degradation; colour change or accumulation of volatiles near the nozzle is an early warning. On production lines with 16–32 cavities, differences in melt delivery between first and last cavity often exceed the effect of the hydrolysis stabiliser, so cavity balance should be measured by short-shot progression at production injection speed.
At room temperature, hydrolytically stabilised PBT/GF30 typically displays mechanical values close to those of standard PBT/GF30. The commercial difference appears after hot-fluid aging, not as an increase in dry tensile strength. The following table collates representative published ranges for 30% glass-filled PBT moulding compounds measured on ISO multipurpose test specimens; the exact lot-specific values for K4560 should be read from the supplier certificate of analysis and should not be inferred from this comparison.
| Property | Test Standard | K4560 Published Typical Direction | Standard PBT/GF30 Typical Direction | Differentiating Note |
|---|---|---|---|---|
| Density | ISO 1183-1 | 1.53 g/cm³ | 1.53 g/cm³ | No significant dry-property difference |
| Tensile stress at break | ISO 527-2 | 105–115 MPa | 100–120 MPa | Overlapping dry values |
| Tensile strain at break | ISO 527-2 | 2.0–3.0% | 2.0–3.0% | Brittle failure mode |
| Flexural modulus | ISO 178 | 6500–7500 MPa | 6500–7500 MPa | Controlled by 30% glass loading |
| Notched Izod at 23°C | ISO 180/1A | 7–9 kJ/m² | 6–10 kJ/m² | Glass-length dependent |
| HDT/A at 1.80 MPa | ISO 75-2 | 195–205°C | 190–210°C | No significant difference |
| Mould shrinkage flow | ISO 294-4 | 0.2–0.4% | 0.2–0.5% | Similar anisotropy |
| Water absorption 24 h | ISO 62 | 0.06–0.10% | 0.06–0.10% | Low; hydrolysis depends on time-temperature |
| Hot-glycol tensile retention at 125°C | USCAR-2 or internal | Improved retention vs standard PBT/GF30; published K4560 data limited | Lower retention; autocatalytic hydrolysis | Primary differentiator |
In connector and sensor housings, electrical performance is evaluated with IEC 60112 for comparative tracking index, IEC 60243-1 for dielectric strength, and IEC 60093 for volume resistivity. Glass-filled PBT grades generally exhibit CTI in the 250–300 V range unless anti-tracking additives are present; specific K4560 CTI values should be requested from the supplier or measured on finished parts. Dielectric strength of 20 kV/mm is typical for dry specimens, but condensing humidity and hot-water immersion can reduce surface resistivity and produce leakage current before bulk mechanical failure occurs.
These electrical properties are not governed solely by the hydrolysis stabiliser. Glass sizing, mineral impurities, mould-release deposits, and humidity history all influence tracking resistance and surface insulation. For parts exposed to salt mist per ISO 9227 or connector durability with current cycling, leakage current and contact resistance should be characterised after 1000 h of damp heat per IEC 60068-2-78. The material is not a substitute for creepage and clearance design; high-voltage connector suitability must be validated at the application voltage, temperature, and pin spacing. If a connector is wave-soldered or reflowed after moulding, residual moisture should be below 0.02% to prevent blistering. Drying after moulding may be required if parts have been stored in uncontrolled humidity prior to soldering.
Global production programmes require documentation that the material contributes to electrical and mechanical function while satisfying controlled-substance obligations. The table lists common compliance routes but is not a legal opinion; regulatory status can change by production location, pigment package, and lot. Each shipment should be covered by a supplier declaration referencing the grade and lot number.
| Requirement | Scope | Verification | K4560 Implication |
|---|---|---|---|
| RoHS 2011/65/EU as amended | Pb, Hg, Cd, Cr(VI), PBB, PBDE at homogeneous material level | EN IEC 63000 technical documentation; XRF screening | Check supplier declaration; no intentional heavy-metal additives assumed |
| REACH EC/1907/2006 | SVHC communications; Annex XVII restrictions | Safety data sheet, SCIP communication if SVHC above 0.1% w/w | Candidate-list status must be confirmed per shipment |
| WEEE 2012/19/EU | EEE material marking and coding | ISO 1043-1 marking | Mark as PBT-GF30 |
| Material designation | PBT, 30% glass-fibre reinforcement | ISO 1043-1 | Nominal glass content 30% |
| Flammability | UL 94 rating | UL yellow card | Confirm K4560-specific rating; glass-filled PBT often HB unless FR additive package is present |
| Food/water contact | Not intended by default | EU 10/2011, FDA 21 CFR | Do not assume compliance for potable-water or food-contact use |
When K4560 replaces an existing standard PBT/GF30 part, the change should be treated as a material requalification, not a simple drop-in substitution. Gate freeze time, weld-line position, ultrasonic weld energy, laser-marking contrast, and dimensional gauges should be revalidated because small changes in melt viscosity or crystallisation rate can alter filling behaviour. Dimensional inspection should be performed after 24 h conditioning at 23±2°C and 50±10% relative humidity in accordance with ISO 291. If warpage is assessed, the measurement fixture should represent the end-use mating condition rather than a flat granite plate alone; fibre orientation and post-mould secondary crystallisation can produce shape changes not captured by simple linear shrinkage.
Melt temperature should not exceed 280°C, and hot-runner manifold temperatures should remain at or below 270°C to limit volatile degradation products that appear as gate blush. For direct comparisons on the same injection moulding machine, processing parameters for K4560 and a standard PBT/GF30 are similar but not identical; shot weight, cushion, and switch-over position should be re-established after the first production trial. Documentation should include actual glass content by ash burn-off per ISO 3451-1, melt volume-flow rate per ISO 1133-1:2022, and any thermal-aging results if the part is under direct engine-compartment radiation. If the application requires laser welding, the upper-layer transmission at 980 nm should be measured, because glass-fibre loading and stabiliser packages can influence scattering and weld strength; not all PBT/GF30 grades are suitable for through-transmission laser welding. The material should not be used in potable-water or food-contact applications without explicit supplier documentation, because the hydrolytic stabiliser package is not automatically approved for those regulated uses.