| HS Code | 247007 |
| Polymertype | Polybutylene terephthalate (PBT) |
| Glassfibercontent | 30% |
| Flameretardant | Yes |
| Ul94rating | V-0 |
| Density | 1.59 g/cm3 |
| Tensilemodulus | 11000 MPa |
| Tensilestrengthatbreak | 120 MPa |
| Elongationatbreak | 2.5% |
| Flexuralmodulus | 10000 MPa |
| Flexuralstrength | 190 MPa |
| Notchedizodimpactstrength23c | 8 kJ/m2 |
| Hdtat1 8mpa | 200 °C |
| Hdtat0 45mpa | 215 °C |
| Meltingtemperature | 225 °C |
| Vicatsofteningtemperature | 210 °C |
| Volumeresistivity | 1E15 ohm·cm |
| Dielectricstrength | 20 kV/mm |
| Moldshrinkage | 0.2-0.5% |
| Melttemperature | 250-280 °C |
| Moldtemperature | 60-100 °C |
| Dryingtemperature | 120 °C |
| Dryingtime | 2-4 h |
As an accredited SABIC VALOX™ PBT+GF30%-FR 420SE0 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | SABIC VALOX™ PBT+GF30%-FR 420SE0 is packed in 25 kg moisture-barrier bags, with 40 bags per 1,000 kg pallet. |
| Container Loading (20′ FCL) | A 20′ FCL is loaded with palletized SABIC VALOX™ PBT+GF30%-FR 420SE0 in 25 kg bags, securely stowed for ocean transport. |
| Shipping | SABIC VALOX™ PBT+GF30%-FR 420SE0 is typically shipped as flame-retardant, glass-fiber-reinforced PBT pellets in moisture-barrier bags, octabins, or bulk containers. Pallets should be kept dry, cool, and protected from heat, sunlight, punctures, and moisture ingress. Handle per SDS; normally non-hazardous with no special dangerous-goods labeling. |
| Storage | Store SABIC VALOX™ PBT+GF30%-FR 420SE0 in a cool, dry, well-ventilated area away from heat, ignition sources, direct sunlight, moisture, oxidizers, acids, and bases. Keep containers tightly closed, labeled, and in original packaging when possible; avoid dust generation. Do not store near food, drink, or animal feed. Follow the safety data sheet and local regulations. |
| Shelf Life | Shelf life is typically two years in original unopened packaging, stored cool and dry, away from sunlight and moisture. |
Inside 12V/48V automotive electrical distribution systems, SABIC VALOX™ PBT+GF30%-FR 420SE0 is assigned to terminal housings and fuse/relay boxes where live-part separation is a thin wall under continuous thermal load. The compliance basis is not a single data sheet entry; it interlocks UL 94 V-0 as documented in the supplier Yellow Card, SAE/USCAR-2 for terminal retention and vibration, EU RoHS 2011/65/EU as amended by (EU) 2015/863, and REACH SVHC declaration. The material is fed as a ready-to-inject pellet, not as a compounding base; the formulation addition ratio is therefore 100 wt% dry virgin 420SE0 at the hopper, with no supplemental flame retardant, no impact-modifier let-down, and no mineral filler. If a color adjustment is unavoidable, a PBT-carrier color masterbatch is held to 2 wt% maximum because higher pigment loading can displace the flame-retardant package at the surface and alter glow-wire behavior. Regrind from sprues and runners may be re-introduced at up to 20 wt% only after the part wall thickness and gate geometry have passed the full UL 94 and USCAR-2 thermal-stress sequence; regrind is not blended into parts carrying a terminal snap-latch that sees repeated insertion/withdrawal. Downstream production is injection molding on multi-cavity connector molds with clamp force typically above 120 tons, a three-zone screw with 2.0–2.5 compression ratio and 20:1 L/D. Pre-drying is mandatory at 120°C for 3–4 h in a desiccant dryer with a dew point at or below -30°C; residual moisture must be below 0.02% because PBT hydrolyzes under melt heat and molecular-weight loss appears first as knit-line cracking at core-pin intersections. Melt temperature is held at 250–270°C, mold temperature at 70–100°C. Production-scale experience has shown gate blush and color streaking around pin valleys when shot-to-shot residence time above 260°C exceeds 8 minutes. Tooling for automotive connector housings requires thermal separation between the hot runner manifold and the cavity plate. If cavity steel temperature exceeds 100°C, the flame-retardant package can form a greasy film on polished surfaces and increase ejected-part drag. Fixed and moving halves are typically run at 70–90°C, with copper-beryllium inserts behind the terminal retention fingers. Short-shot studies establish the transfer position at 95% fill; final packing at 55–65 MPa for 1.5–2.5 s is sufficient for most 0.8–1.2 mm walls, but longer packing at high speed causes flash because the glass-filled flow front freezes quickly. Dimensional audit data from multi-cavity production show cavity-to-cavity variation in pin-to-pin pitch of ±0.04 mm is achievable only if the manifold is naturally balanced and regrind percentage is stable. Terminal product types include engine ECU connector housings, 48V power distribution junction boxes, relay sockets, and fuse-box bases.
Because miniature circuit breaker and residual current device housings are live-part barriers, the molding department treats them as a glow-wire validation exercise rather than a dimensional part only. The compliance basis includes IEC 60695-2-12 glow-wire flammability index at the end-product threshold required by IEC 60898-1 and UL 489, IEC 60695-2-13 glow-wire ignition temperature at the specified end-product wall section, and IEC 60112 comparative tracking index; final approval attaches to the complete breaker, not to the resin alone. VALOX 420SE0 is introduced at 100 wt% as-supplied pellet feed; no char former, no nitrogen-phosphorus intumescent, and no halogen carrier are added on the molding floor. If a specific color is required, the formulation ratio is 98 wt% 420SE0 to 2 wt% PBT-carrier masterbatch. Colorants with metallic stearate release packages are excluded because they can reduce tracking resistance and leave deposits on cavity vents. Downstream injection molding for MCB bases uses hot runner systems with natural-balanced manifolds and valve gates to avoid dead spots. Melt temperature is set at 250–265°C; mold temperature at 60–90°C. Parting-line vent depth is limited to 0.015–0.020 mm because the flame-retardant gas byproducts must escape without producing flash. Plant-scale production records show that core-shift-induced wall-thickness variation below 1.0 mm is the primary cause of glow-wire failure at screw bosses, not resin lot variation. Because glass-fiber orientation at the gate determines warpage in long MCB frames, the gate is located on a nonfunctional end wall and sized at 1.0–1.2 mm for a wall thickness of 1.5–2.0 mm. The hot runner manifold temperature is set 5–10°C above the nozzle temperature to avoid premature solidification at the valve pin. After gate seal, the holding phase is terminated based on cavity pressure rather than fixed time; production data show that extending hold beyond gate seal does not reduce sink at bosses but increases residual stress at the rail. Terminal product types include MCB cover shells, RCD base frames, contactor arc-chamber side walls, and auxiliary contact housings.
Compliance with IEC 60335-1 for unattended appliance control boards imposes a different failure criterion than flame propagation: it is the ability to hold a live terminal under stabilized mechanical force after abnormal heating. VALOX 420SE0 is molded into power-control modules, relay sockets, and sensor brackets with a feed ratio of 100 wt% dry virgin material; regrind use is capped at 15 wt% in this sector because appliance OEMs require tighter color consistency and lower volatile content after multiple heat histories. The relevant standards are IEC 60335-1 clause 30, IEC 60695-10-2 ball pressure at 125°C, and IEC 60112 comparative tracking index for board spacers mounted below a live PCB. A significant production constraint is that the grade must not be diluted with unfilled PBT to improve surface gloss; a glass-content shift below 30% reduces rigidity and can change the UL 94 classification at the same wall section. No dilution ratio above 0% is accepted without full UL file review. Downstream production is multi-cavity straight-pull molding with robot sprue pick, dry-cycle check, and mold exhaust through porous sintered vents to remove volatile flame-retardant byproducts. Melt temperature is controlled at 250–270°C; mold temperature at 70–100°C; screw speed at 80–120 rpm. Field experience shows sink marks at boss bases become detectable from differential shrinkage when cavity pressure drops below 60 MPa, so packing is held at 70–80 MPa for 2–4 s. Terminal product types include washing machine motor-control housings, dishwasher relay brackets, induction hob control-box frames, and coffee machine power modules.
For electric motor coil bobbins and brush-card frames, the material must survive magnet-wire tension during winding and thermal aging in a Class F insulation system. Compliance is anchored to UL 1446 and IEC 61857-1, with IEC 60085 thermal class indexing; final approval is on the complete motor, not on the isolated plastic. VALOX 420SE0 is processed as a neat pellet feed at 100 wt% virgin; no glass roving recompounding and no impact-modifier dilution are allowed because a 5 wt% unfilled PBT side stream can increase flange warpage and reduce dielectric distance between winding layers. For thin-wall bobbins below 0.8 mm, regrind is limited to 10 wt% because regrind lot-to-lot variation in residual glass length changes flow orientation and flange flatness. The downstream process is injection molding with center-gated or diaphragm-gated cavities, mold temperature 80–100°C, and melt temperature 245–265°C. Gate location is positioned away from the flange-to-barrel transition because flow hesitancy in that region creates a residual strain gradient. Steel core pins with draft below 0.5° increase extraction drag and contribute to flange cracking during automated bobbin unloading. Terminal product types include solenoid coil bobbins, shaded-pole motor bobbins, brush-card supports for portable power tools, and stepper motor insulating frames.
In EV charging gun internal housings, the plastic is not the outer UV-stabilized shell but the inner current-carrying support that positions contact pins and the temperature-sensor well. The compliance basis includes IEC 62196-1 for mode 2/3 vehicle connectors, UL 2251 for North American plugs, and EN 50620 for cable assemblies; internal insulation also must satisfy IEC 60695-2-11 glow-wire requirements at the final product level, though published data for this specific long-aging configuration in 420SE0 is limited and end-product validation is mandatory. The formulation addition ratio is 100 wt% virgin 420SE0 pellets with no post-extraction regrind, because pin-retention wall sections are below 1.5 mm and recycled material can shift the coefficient of thermal expansion enough to loosen press-fit silver-plated copper pins after thermal cycling. If a color masterbatch is used, the ratio is 98 wt% resin to 2 wt% masterbatch, and the masterbatch must be halogen-free and free of talc. Downstream production is valve-gated injection molding with sequential filling from the pin area toward the cable strain-relief overmold. Melt temperature is held at 250–265°C; mold temperature at 70–100°C; holding pressure at 60–80 MPa. The principal production bottleneck is internal air trapping at pin-support ribs; it is relieved by sintered-vent inserts and by reducing filling speed in the final 30% of stroke. Terminal product types include charge gun inner frames, Type 2 pin carriers, temperature-sensor holders, and DC fast-charge inlet connector bodies for vehicle-side assemblies.
When high-power LED driver and ballast enclosures are specified with a 30% glass-reinforced flame-retardant PBT, the critical requirement outside the printed-circuit board is dimensional stability under capacitor heat, not ignition resistance alone. The applicable compliance package includes UL 8750, IEC 61347-1, and UL 94 V-0 on the plastic enclosure; the material is also assessed for glow-wire resistance under IEC 60695-2-11 when the enclosure is positioned above the PCB. Processing uses 100 wt% virgin VALOX 420SE0 pellet feed. If in-plant regrind from runner systems is reused, it is kept at 20 wt% maximum and only in non-optical, non-sealing enclosure walls because one pass through a 20:1 L/D screw changes the residual glass-fiber length distribution and alters surface roughness and heat-deflection behavior at thin boss features. Downstream production is injection molding with mold temperature 70–100°C and melt temperature 250–270°C; the process window is tight around the upper limit because the flame-retardant additive package decomposes above the 270°C upper melt-temperature limit, causing silver streaks at the gate and a drop in Izod impact. Cavities are run with vent depths of 0.01–0.02 mm. Terminal product types include slim LED driver enclosures, ballast housings, module covers for commercial lighting, and emergency-lighting battery carrier frames.
Competitive SABIC VALOX™ PBT+GF30%-FR 420SE0 prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
SABIC VALOX™ PBT+GF30%-FR 420SE0 is a 30% glass-fibre reinforced, flame-retardant polybutylene terephthalate injection moulding grade. The model designation identifies the nominal glass loading, the flame-retardant package, and the SE0 self-extinguishing class associated with thin-wall UL 94 performance. Published manufacturer data list the density at 1.63 g/cm³ under ISO 1183, tensile stress at break at 125 MPa under ISO 527-1/-2, tensile strain at break at 2.0%, flexural modulus at 10,500 MPa under ISO 178, and notched Izod impact strength at 10 kJ/m² at 23 °C under ISO 180/1A. The grade is specified for electrical connectors, relay bases, motor housings, and enclosure components requiring stiffness, dimensional reproducibility, and defined flame-retardant response under IEC 60695-11-10.
| Property | Test method | Typical value |
|---|---|---|
| Specific gravity | ISO 1183 | 1.63 |
| Tensile stress at break | ISO 527-1/-2 | 125 MPa |
| Tensile strain at break | ISO 527-1/-2 | 2.0% |
| Flexural stress at break | ISO 178 | 180 MPa |
| Flexural modulus | ISO 178 | 10,500 MPa |
| Notched Izod impact at 23 °C | ISO 180/1A | 10 kJ/m² |
| Heat deflection temperature at 1.8 MPa | ISO 75-2/Ae | 205 °C |
| Vicat softening temperature B/120 | ISO 306 | 215 °C |
| UL 94 rating | IEC 60695-11-10 | V-0 at 0.75 mm |
Mould shrinkage in the flow direction is published between 0.2% and 0.5%. The measured value is influenced by gate geometry, wall thickness, melt temperature, mould temperature, and pack pressure. For flat housings with ribs and bosses, shrinkage anisotropy must be included in the tool-design simulation rather than assumed from a single generic coefficient.
The glass-fibre reinforcement reduces melt flow relative to unfilled PBT. Published melt volume-flow rate for 420SE0 is reported in the range of 8–15 cm³/10 min at 250 °C with 2.16 kg load under ISO 1133-1, depending on batch moisture and thermal history. Capillary rheometry under ISO 11443 shows pronounced shear-thinning above 1,000 s⁻¹, which permits thin-wall filling when gate shear rates are adequately high. However, the low-flow characteristic limits the practical wall-section range: very long flow paths below 0.4 mm generate excessive pressure loss and glass-fibre orientation streaks at the gate.
On injection moulding machines with screw diameters from 25 mm to 45 mm, the recommended melt temperature is 250 °C to 270 °C. Barrel temperature settings typically progress from 240 °C in the rear zone to 260 °C at the nozzle. The mould temperature should be held between 80 °C and 100 °C for thin-wall parts. Mould temperatures below 60 °C shorten cycle time but reduce crystallinity development and may produce post-mould shrinkage exceeding 0.15% over 48 h. The practical stable melt-temperature band is narrower than the general PBT range because the flame-retardant package degrades above 270 °C, while glass bundle dispersion becomes incomplete below 245 °C. Closed-loop nozzle and hot-runner temperature control is therefore specified.
Screw geometry should be low-compression with a length-to-diameter ratio of 20:1 to 25:1 and a check ring designed for glass-filled materials. The shot size should not exceed 70% of barrel capacity. Insufficient plastication leads to unmelted glass bundles that orient in the gate area and create surface streaks. Hot-runner manifold temperatures should not exceed 260 °C, and manifold residence time should remain below 3 min to avoid flame-retardant decomposition and black-spec formation. Cold-runner tools with heated sprue bushings are preferred for thin-wall connectors because they limit the residence time of the glass-filled melt in the delivery system.
Moisture control is the primary processing boundary. PBT ester linkages undergo hydrolysis at melt temperature when residual pellet moisture exceeds 0.02%. The pellets are dried at 120 °C for 4 h in a desiccant dryer with a dew point below −30 °C. At ambient relative humidity above 60%, closed-loop hopper conveying is required. Moisture analysis capable of resolving 0.005% is used for verification. Extended drying above 8 h at 120 °C produces oxidative yellowing and measurable loss in tensile strain at break. Regrind addition is structurally limited to 25% unless notched impact retention is verified, because repeated thermal and shear history reduces glass-fibre length and impact strength.
The flame-retardant system in 420SE0 is halogenated. Thermal decomposition above 280 °C releases acidic decomposition products; local exhaust ventilation and periodic tool-vent cleaning are therefore required in production. Under IEC 60695-11-10, the grade is rated V-0 at 0.75 mm. At 1.5 mm and greater, 5VB performance is achievable, but the rating is assembly-thickness dependent and is influenced by gate location, weld lines, glass orientation, and venting. Thin ribs below 0.4 mm may exhibit inconsistent afterflame times because glass fibres can act as combustion wicking paths if flame-retardant dispersion is locally depleted by improper drying or excessive barrel residence time.
Comparative tracking index is typically 250 V under IEC 60112. The grade is used in electrical enclosures where a defined glow-wire performance and creepage resistance are required, but the exact glow-wire result depends on final wall thickness and colour. Thermogravimetric analysis under ISO 11358-1 shows that the flame-retardant system lowers the onset of the principal thermal decomposition step relative to non-FR PBT. This behaviour defines the upper processing temperature boundary: sustained melt temperatures above 270 °C degrade the FR synergist and produce measurable loss of V-0 performance after regrind.
Barrel residence time at 270 °C must remain below 6 min. At residence times above 10 min the melt colour shifts and the notched impact strength declines by more than 20% in published ageing trials. The combination of glass fibre and halogenated FR chemistry also makes tool wear more aggressive than with unfilled PBT; hardened steels or bimetallic barrels and screws are specified for production runs above 500,000 cycles.
The principal difference from unfilled PBT is the increase in stiffness and elevated temperature load-bearing capacity. Unfilled flame-retardant PBT has a heat deflection temperature under 1.8 MPa of approximately 60 °C; 420SE0 raises that value to 205 °C. The flexural modulus is approximately four times higher than unfilled PBT. The trade-off is reduced melt flow and increased anisotropy in mould shrinkage.
| Property | Unfilled FR PBT | Non-FR GF30 PBT | 420SE0 |
|---|---|---|---|
| Specific gravity, ISO 1183 | 1.41 | 1.53 | 1.63 |
| Tensile stress at break, ISO 527-1/-2 | 55 MPa | 120 MPa | 125 MPa |
| Flexural modulus, ISO 178 | 2,500 MPa | 9,000 MPa | 10,500 MPa |
| Heat deflection temperature at 1.8 MPa, ISO 75-2/Ae | 60 °C | 210 °C | 205 °C |
| UL 94 rating, IEC 60695-11-10 | V-0 at 1.5 mm | HB | V-0 at 0.75 mm |
| Mould shrinkage flow direction | 1.5–2.0% | 0.2–0.5% | 0.2–0.5% |
Compared with non-FR GF30 PBT, 420SE0 adds the V-0 flame-retardant capability with only a modest density increase and similar tensile strength. The principal engineering trade-off is elongation and impact. Non-FR GF30 PBT typically displays higher notched Izod impact strength than the flame-retardant version because the FR package concentrates stress at the glass-matrix interface. Flow length is also lower in 420SE0 than in non-FR GF30 PBT at identical injection pressure, so gate quantity and runner sizing require adjustment when a tool is converted from a non-FR grade.
Against unfilled FR PBT, 420SE0 is less suitable for extremely thin-wall connectors with long flow paths, because the glass fibre lowers melt flow. Unfilled FR PBT can fill sections below 0.3 mm more readily, but its low flexural modulus and low HDT make it unsuitable for structural electrical housings. The choice between unfilled FR PBT and 420SE0 therefore depends on whether the part carries mechanical load or is primarily an insulating carrier.
In metal replacement, the coefficient of linear thermal expansion is approximately 2.5 × 10⁻⁵ K⁻¹ in the flow direction and 7.0 × 10⁻⁵ K⁻¹ transverse under ISO 11359-2. The anisotropy is significant and must be incorporated into warpage simulation. The material eliminates secondary machining and supports insert moulding, but the designer must accept a lower continuous-use temperature than aluminium. Published relative thermal index values for the electrical and mechanical without impact categories are typically 130 °C and 140 °C under UL 746B; these values require confirmation for the specific colour and minimum wall thickness of the moulded part.
In humid service, 420SE0 absorbs approximately 0.06% by mass after 24 h immersion under ISO 62. A typical 30% glass-filled flame-retardant PA66 grade absorbs above 0.8% at 50% relative humidity, with subsequent loss in modulus and dielectric strength. The lower moisture uptake of PBT maintains more stable dimensional and electrical performance in electrical terminals exposed to condensation or washdown. This is a primary reason 420SE0 is specified in place of polyamide for connector housings and relay bases in humid electrical enclosures.
The principal operational boundary is hydrolytic ageing. 420SE0 is not recommended for continuous immersion in hot water above 60 °C. Hydrolysis of the PBT ester backbone reduces tensile strength at a rate that may not be captured by short-term data. In such environments, a PPS or PBT/PET blend is substituted. For outdoor enclosures, published data for long-term UV exposure specific to 420SE0 are limited; black or UV-stabilised formulations are preferred where sustained irradiance exceeds 500 W/m² in ISO 4892-2 testing. Dimensional stability should also be validated by a 48 h room-temperature ageing study before final tool dimensions are fixed, because post-mould shrinkage of glass-filled PBT can be anisotropic and time-dependent.
Processing on production-scale equipment shows that tool venting is critical. On multicavity connector tools with 32 or more cavities, vent depth should not exceed 0.02 mm to avoid flash while still allowing discharge of decomposition gases from the flame-retardant package. Injection speed should be limited to prevent jetting and visible fibre orientation at the gate; sequential valve gating is used for long flat housings to maintain a stable melt front. The practical barrel temperature window on continuous operation is 250 °C to 270 °C, with the nozzle temperature set 5 °C below the melt temperature to control drool. Screw rotation should be limited to 60–80 rpm on small machines and 25–40 rpm on machines above 200 t clamp force to limit glass-fibre attrition. Injection pressure at the transfer point is typically 70–90 MPa for thin-wall sections, with hold pressure maintained at 70% of peak fill pressure for 8–12 s to control gate sink. Published data for this specific configuration are limited in academic literature, but these ranges are consistent with manufacturer technical bulletins for glass-filled flame-retardant PBT.