Sabic Valox Pbt Gf30 865

SABIC VALOX™ PBT+GF30% 865

    • Product Name: SABIC VALOX™ PBT+GF30% 865
    • Factroy Site: Yinchuan, Ningxia, China
    • Price Inquiry: sales8@ascent-chem.com
    • Manufacturer: Ascent Petrochem Holdings Co., Limited
    • CONTACT NOW
    VTB
    Specifications
    HS Code 869580
    Material Type Polybutylene terephthalate (PBT)
    Glass Fiber Content 30%
    Flame Retardancy UL94 V-0
    Density approx. 1.53 g/cm³
    Tensile Modulus approx. 10,000 MPa
    Tensile Strength At Break approx. 120 MPa
    Elongation At Break approx. 2.5%
    Flexural Modulus approx. 9,000 MPa
    Notched Izod Impact Strength approx. 80 J/m
    Hdt At 1 82 Mpa approx. 200 °C
    Water Absorption At 23 C 24 H approx. 0.06%
    Molding Shrinkage approx. 0.2–0.5%
    Dielectric Strength approx. 20 kV/mm
    Volume Resistivity >1E15 ohm·cm

    As an accredited SABIC VALOX™ PBT+GF30% 865 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.

    Packing & Storage
    Packing SABIC VALOX™ PBT+GF30% 865 is supplied in 25 kg moisture-barrier bags, palletized and clearly labeled for industrial handling.
    Container Loading (20′ FCL) 20′ FCL container loaded with palletized 25 kg bags of SABIC VALOX™ PBT+GF30% 865, securely stowed for export shipment.
    Shipping SABIC VALOX™ PBT+GF30% 865 is shipped as non-hazardous, moisture-sensitive thermoplastic pellets (polybutylene terephthalate with 30% glass fiber) in sealed bags or octabins. It is not regulated for transport under DOT/IMDG/IATA. Store dry, avoid direct sunlight, and protect packaging from damage.
    Storage Store SABIC VALOX™ PBT+GF30% 865 in a cool, dry, well-ventilated area, away from direct sunlight, heat, flames, and oxidizing agents. Keep original containers sealed, labeled, and protected from moisture, dust, and contamination. Avoid prolonged high humidity, maintain stable temperature, and use oldest stock first. Prevent physical damage to packaging.
    Shelf Life Shelf life is 24 months from manufacture when stored unopened in original packaging, dry, below 30°C, and away from sunlight.
    Application of SABIC VALOX™ PBT+GF30% 865

    In underhood connector bodies moulded from SABIC VALOX™ PBT+GF30% 865, the first production control point is residual moisture before plastication, because hydrolytic degradation at melt temperatures above 250 °C shortens polymer chains and reduces terminal retention force. A closed-loop desiccant drier operating at a dew point below -30 °C and an air temperature of 120 °C for 4 h is applied to pellet feedstock; the target moisture content is below 0.02% by Karl Fischer titration. Injection moulding is carried out on a reciprocating-screw machine with an L/D ratio between 18:1 and 22:1, using a bimetallic barrel and a hardened screw flight to resist wear from 30% glass fiber. Barrel zones are profiled from 245 °C at the feed throat to 265 °C upstream of the nozzle, with the nozzle maintained at 255–270 °C and the melt temperature verified by an air shot before production. The mould wall is held at 80–100 °C, and injection pressure is typically 80–120 MPa, with pack pressure set to compensate for shrinkage anisotropy measured at 0.2–0.6% in the flow direction and 0.5–1.0% transverse on 60 mm × 60 mm × 2 mm plaques per ISO 294-4. Multi-pin connector bodies present a weld-line risk because glass fibers orient along convergent flow fronts and reduce tensile strength at the knit line to roughly 55–70% of the un-welded value; gates are therefore relocated to move weld lines away from latch arms, pin retention features, and snap-fit engagement surfaces. Electrical connector validation for engine-bay use follows SAE/USCAR-2 mechanical and electrical cycles, with humidity exposure and thermal shock conducted according to ISO 16750-4, and terminal retention force measured on the retention lance rather than the housing wall. End articles include ECU header frames, camshaft-position sensor sockets, throttle-body connector bodies, and ISO relay housings. Long-term thermal aging is assessed through UL 746B relative thermal index data; for 30% glass-filled PBT the electrical RTI commonly falls in the 140–155 °C band, but the material is not specified for continuous peak contact temperatures above 180 °C or for direct contact with hot glycol at temperatures above 80 °C. Shot size is maintained between 40% and 70% of barrel capacity, with a screw cushion of 3–6 mm to maintain consistent pack pressure at the gate.

    What Lowers Comparative Tracking Index in E/E Distribution Enclosures?

    Miniature circuit breaker housings, relay bases, and DIN rail terminal blocks made from VALOX™ PBT+GF30% 865 must satisfy creepage and clearance spacing defined in IEC 60664-1; this shifts control from mechanical strength alone to surface tracking resistance under polluted conditions. Comparative tracking index is measured per IEC 60112 with solution A, and 30% glass-reinforced PBT typically exhibits a CTI value in the 250–300 V range when tested on virgin moulded plaques. The process boundary is regrind fraction: production trials show that adding more than 20 wt% clean, desiccant-dried regrind raises the probability of exposed glass fibers at the melt front and reduces tracking resistance; for components carrying a rated impulse withstand voltage below 4 kV, regrind is usually limited to 15 wt% to preserve surface insulation consistency. Valve-gated hot-runner sequences are used in long rectangular enclosures because the pack and hold phase must compensate for differential shrinkage between the outer wall and the terminal partition; sequential opening of valve pins is timed to prevent gas traps at the far end of the cavity. The mould temperature is maintained at 90–110 °C in this case, deliberately above the PBT glass transition, to raise crystallinity and improve surface hardness, but the higher mould temperature increases cycle time by 10–20% relative to a cold-runner tool. Components are tested for glow-wire ignition temperature per IEC 60695-2-13 only on the final wall thickness because the grade is classified UL 94 HB and is not a flame-retardant compound. End products include MCB bases for rail-mounted circuit protection, relay sockets, contactor base plates, and DIN rail terminal partition walls. Field experience from multi-cavity production of MCB housings indicates that the highest rejection mode is fill imbalance caused by fiber orientation differences between cavities when the runner system is not geometrically balanced; a standard 8-cavity cold runner can show cavity-to-cavity weight variation above 0.5% unless adjuster pins are machined. Injection speed is therefore set between 60 mm/s and 120 mm/s at the screw face, with hold pressure time sufficient to seal the gate, usually 6–10 s depending on wall thickness.

    Insert moulding of brass blades and terminal posts in industrial motor terminal boards begins with insert preheating at 120–140 °C immediately before insert moulding to reduce the thermal shock and differential contraction that can create microcracks around the metal-polymer boundary. The PBT+GF30% compound is dried at 120 °C for 4 h; barrel settings are kept at 250–265 °C and the melt residence time is restricted to less than 5 min at these temperatures to limit polymer chain decomposition. Injection velocity is reduced during the first 20–30% of fill to prevent displacement of thin brass blades, then increased to 80–110 mm/s for the remaining cavity volume. Post-mould thermal conditioning at 120–130 °C for 1–2 h is applied to components that must pass vibration tests class 3M2 per IEC 60721-3-3, because annealing relieves retained stress and stabilizes subsequent dimensional movement. Electrical clearances are dimensioned to IEC 60664-1 pollution degree 3, and the terminal board is subjected to dielectric withstand testing at 2,000 V AC for 1 min if working voltage is below 250 V. End products include motor junction box terminal boards, carbon brush holder plates, and high-voltage partition walls for servo motor drives. The main processing incompatibility is with release agents containing silicone or hydrocarbon oils, which can migrate into the surface and degrade adhesion of potting compounds applied later; only dry-film mold release agents approved for electrical insulation are permitted.

    When IEC 60320 Inlet Bodies Undergo 850 °C Glow-Wire Verification

    Appliance inlet bodies and switch housings moulded from VALOX™ PBT+GF30% 865 must be evaluated for end-product glow-wire performance under IEC 60695-2-11, because the base resin is a non-flame-retardant HB grade and results depend strongly on final wall thickness, colorant chemistry, and regrind content. The process window is narrowed when a component must resist ignition or self-extinguish after the glow wire is removed at 850 °C for 30 s; under these conditions the moulder reduces regrind to 10 wt% maximum and avoids masterbatches based on polyethylene wax carriers that can act as fuel. Melt temperature is kept in the lower portion of the processing range, 250–260 °C, to reduce formation of low-molecular-weight degradation species, while mould temperature is raised to 100 °C to produce a high-crystallinity skin. Injection speed is set to 70–100 mm/s and back pressure to 3–6 bar hydraulic, with screw pullback decompression kept below 3 mm to avoid air entrapment and surface silver streaks. Dimensional compliance for IEC 60320-1 inlet bodies includes pin spacing and shroud depth checks on a coordinate measuring machine after 24 h conditioning at 23 °C and 50% relative humidity. The grade is suitable for C14 inlet bodies, coffee machine terminal covers, and appliance switch actuators, provided that the approval test is conducted on the moulded component rather than inferred from resin data, because published data for this specific configuration is limited. Long-term contact with steam or boiling-water spray must be prevented; hydrolytic degradation accelerates above 60–80 °C in aqueous environments.

    IEC 60238 Lampholder Shells and Thermal Accumulation at the Centre Contact

    To meet IEC 60238, E14 and E27 lampholder shells produced from the 30% glass-filled PBT grade are tested for mechanical strength, heat resistance, and electrical insulation after thermal conditioning. Thermal accumulation at the centre contact rivet is the principal long-term failure driver, because a poorly heat-sinked LED retrofit lamp can raise local plastic temperature above the mechanical RTI of the material; thermocouple measurements on production lampholders show that sustained shell temperatures must remain below 140 °C to avoid oxidation embrittlement and loss of spring contact retention. Moulding is performed with a melt temperature of 255–270 °C and a mould wall temperature of 90–110 °C to obtain a glossy, dimensionally stable shell; post-mould annealing at 130 °C for 1 h is applied where maximum thread roundness stability is required. The feedstock is dried to below 0.02% moisture, and regrind is held below 20 wt% because lampholder threads are knit-line prone and excessive regrind worsens thread root notching. End products include E14/E27 lampholder bodies, MR16 pin-base holders, and terminal sleeves for linear fluorescent lampholders tested to IEC 60838. Since the material is not flame-retardant, the end-product glow-wire test is conducted at 650 °C or 750 °C depending on final product standard, and the result is validated on the moulded shell wall thickness rather than a standardized plaque.

    Impact-Modified Alternatives Are Not Required for Every Tool Housing Rib

    Power tool brush housings, trigger frames, and motor end caps moulded from VALOX™ PBT+GF30% 865 rely on flexural modulus near 8,500 MPa per ISO 178 and tensile strength above 120 MPa per ISO 527-1/-2 to stabilize bearing bores and gear alignment under load. The trade-off is notched impact sensitivity; for components subject to IEC 60068-2-75 impact hammer tests, the design must avoid sharp internal corners with radii below 0.5 mm, and gate location is selected so that weld lines do not cross load-bearing rib roots. Moulding uses a screw with a compression ratio of 2.5:1 to 3.0:1, melt temperature 250–265 °C, and mould temperature 80–100 °C. Because short glass fibers align with flow, the moulded part develops anisotropic shrinkage of 0.3–0.6% parallel and 0.8–1.2% perpendicular to flow; gear housing bores are therefore positioned perpendicular to the primary glass orientation where possible. Regrind is allowed up to 20 wt% in non-structural covers, but brush covers with snap latches are moulded from virgin material only because the notch sensitivity increases with fiber-length attrition. End products include angle grinder brush covers, drill trigger switch frames, and dust-blow motor shrouds. Published data for this specific configuration is limited in impact fatigue life, so EN IEC 62841-1 drop tests and impact tests are performed on complete tools before production release.

    For HVAC damper actuator gear housings, the key specification is dimensional stability across a temperature range from -20 °C to 70 °C, not thermal endurance. VALOX™ PBT+GF30% 865 is dried at 120 °C for 4 h; mould temperature is 80 °C and regrind is limited to 20 wt%. Components are checked for gear-tooth total profile deviation under IEC 60730-1 functional tests. Published data for this specific configuration is limited.

    Free Quote

    Competitive SABIC VALOX™ PBT+GF30% 865 prices that fit your budget—flexible terms and customized quotes for every order.

    For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.

    We will respond to you as soon as possible.

    Tel: +8618005193850

    Email: sales8@ascent-chem.com

    Inquiry

    Get Free Quote of Ascent Petrochem Holdings Co., Limited

    Flexible payment, competitive price, premium service - Inquire now!

    Certification & Compliance
    More Introduction

    SABIC VALOX™ PBT+GF30% 865 is a 30% by mass glass-fiber-reinforced polybutylene terephthalate injection-molding grade. Under ISO 1043-1 the material is designated PBT-GF30; the matrix is a semicrystalline polyester and the reinforcement is E-glass fiber. Density measured according to ISO 1183-1:2019 is typically 1.53 g/cm³ to 1.55 g/cm³. Melt volume-flow rate determined at 250 °C and 2.16 kg in accordance with ISO 1133-1:2022 is commonly reported from 9 cm³/10 min to 14 cm³/10 min. The grade is normally classified HB under UL 94; flame-retardant PBT-GF30 alternatives must be selected when V-0 or V-1 ratings are required. Current UL Yellow Card values should be consulted for color- and thickness-specific ratings. The product is distinguished from unfilled PBT by higher modulus, higher heat-deflection temperature, and lower mold shrinkage, but it trades away part of the room-temperature notched impact response and some chemical compatibility in exchange.

    What Limits the Drying and Melt-Processing Window for VALOX 865?

    Moisture control before molding is mandatory because the ester linkages of PBT hydrolyze in the melt. Residual moisture above 0.02 wt%, measured by ISO 15512:2019, causes chain scission that reduces melt viscosity and tensile strength. In severe cases, molded surfaces show splay, and screw recovery time drifts outside control limits. Desiccant-bed drying at 110–120 °C for 4–6 h with a closed-loop hopper and air-stream dew point of -30 °C to -40 °C is required. Dried pellets should transfer to the feed throat through dry-air or nitrogen-purged conveying lines. When ambient relative humidity exceeds 60%, transfer time beyond 2 h can reintroduce 0.005–0.01 wt% moisture before the feed throat.

    Melt temperature at the nozzle is normally maintained between 250 °C and 270 °C. A barrel profile from 240–250 °C at the rear zone to 255–265 °C in the metering zone is used. Mold temperature should be controlled between 60 °C and 100 °C; temperatures below 60 °C reduce crystallization rate and create amorphous skin layers that lower effective heat resistance and chemical resistance, while temperatures above 100 °C add cycle time without a proportional improvement in properties. Residence time at melt temperature should not exceed 8 min because prolonged hold above 280 °C produces thermal decomposition, discoloration, and release of volatile degradation products. Back pressure of 0.3–0.7 MPa is sufficient to maintain shot consistency without excessive glass-fiber attrition.

    Recommended processing parameter ranges for SABIC VALOX™ PBT+GF30% 865
    ParameterRangeMethod or equipment
    Pre-drying temperature110–120 °CDesiccant-bed dryer, closed-loop hopper
    Pre-drying time4–6 hFrom sealed containers; longer for moist material
    Residual moisture<0.02 wt%ISO 15512 Karl Fischer/coulometric titration
    Nozzle melt temperature250–270 °CIR pyrometer or needle thermocouple
    Mold temperature60–100 °CThermolator or manifold coolant
    Back pressure0.3–0.7 MPaHydraulic or transfer setting
    Maximum residence time<8 minShot-consistent cycle timer
    Screw L/D18–22General-purpose injection screw

    Rheological behavior is strongly shear-thinning. At 250 °C, apparent viscosity at 1000 s⁻¹ is commonly 80–150 Pa·s, and at 10,000 s⁻¹ it falls to 30–60 Pa·s. Injection unit screws with L/D 18–22, compression ratio 2.5:1–3.5:1, and a non-restrictive non-return valve preserve fiber length. Restrictions below 1.5 mm in hot runners or valve gates can cause fiber attrition that reduces tensile strength by 5–15%. The glass-reinforced compound is produced on co-rotating twin-screw extruders with L/D 40:1 and side-fed glass; vacuum venting at -0.08 MPa removes volatiles before pelletizing.

    Short-term mechanical properties measured on injection-molded Type 1A specimens separate the 30% glass-fiber formulation from unfilled and low-glass PBT compounds. Tensile stress at break under ISO 527-2/5 typically falls between 115 MPa and 135 MPa, while tensile strain at break remains from 2.0% to 3.5%, a brittle failure mode controlled by glass-matrix debonding. Flexural modulus under ISO 178 is commonly reported between 8500 MPa and 9500 MPa, approximately three to four times the 2300–2700 MPa of unfilled PBT. Notched Izod impact strength under ISO 180/A at 23 °C is typically 8–12 kJ/m². At -30 °C the value declines to 6–8 kJ/m², a critical boundary for snap-fit and thin-wall bosses.

    Typical comparative property ranges for injection-molded PBT grades
    PropertyTest methodUnfilled PBTPBT+GF15VALOX PBT+GF30% 865Impact-modified PBT+GF30
    DensityISO 1183-11.30–1.32 g/cm³1.42–1.45 g/cm³1.53–1.55 g/cm³1.45–1.50 g/cm³
    Tensile stress at breakISO 527-2/550–60 MPa90–100 MPa115–135 MPa95–110 MPa
    Flexural modulusISO 1782300–2700 MPa5000–6000 MPa8500–9500 MPa6500–7500 MPa
    HDT/A at 1.8 MPaISO 75-1/250–60 °C175–185 °C200–215 °C190–205 °C
    Notched Izod at 23 °CISO 180/A4–6 kJ/m²5–7 kJ/m²8–12 kJ/m²12–18 kJ/m²
    Mold shrinkage, flowISO 294-41.4–1.8%0.6–0.8%0.4–0.6%0.5–0.7%

    Ranges represent typical injection-molded data for natural grades; color concentrates, recycled content, and tooling geometry shift the values. Verification on production specimens is required before final part approval.

    Electrical Insulation and Thermal Aging Behavior in Connector Applications

    Volume resistivity determined under IEC 62631-3-1 is typically 10¹³–10¹⁵ Ω·cm at 23 °C on conditioned plaques. Dielectric strength under IEC 60243-1 at 2.0 mm thickness is commonly reported between 15 kV/mm and 20 kV/mm, but glass-rich weld lines and heavy flow-pattern variation reduce the local breakdown threshold. Comparative tracking index under IEC 60112 is commonly 250–300 V at 100 drops of solution A, placing the grade in tracking class 2. Long-term thermal aging under UL 746B often supports an electrical relative thermal index near 130 °C, with the exact value dependent on color, thickness, and end-use test program.

    Connector and socket designs use the glass reinforcement to reduce creep and to maintain terminal retention at elevated temperatures. However, glass-fiber orientation creates anisotropic dielectric and mechanical behavior. Weld lines can reduce tensile strength by 30–50% relative to bulk material and may reduce dielectric strength by 10–20% where fibers align parallel to the electric field. Gate location should place weld lines away from high-voltage barriers and terminal crush ribs. Wall thickness below 0.8 mm can produce resin-rich or glass-depleted sections that lower tracking resistance and dimensional repeatability.

    Polybutylene terephthalate ester linkages are hydrolytically sensitive in hot aqueous media. Continuous exposure of molded parts to water above 80 °C or steam is not recommended because hydrolysis causes surface chalking, loss of tensile strength, and cracking. The compound resists aliphatic hydrocarbons, gasoline, diesel, lubricating oils, and alcohols at 23–60 °C. Strong alkalis, hot concentrated acids, ketones, and chlorinated solvents can attack or stress-crack the material. Fuel-system parts exposed to methanol blends above 15 vol% should be validated on finished parts; published data for this specific grade under aggressive gasoline-methanol mixtures is limited. Incompatibility with primary amines is a documented boundary: prolonged contact with amine-cured epoxy potting compounds or amine-based lubricants at service temperatures above 60 °C can accelerate aminolysis and reduce molecular weight. Validation of assembled chemical contact is performed using static-strain fixtures under ISO 175 or equivalent environmental stress-cracking protocols.

    Short-term paint-bake excursions to 180 °C for 30 min are acceptable only if parts are unfixtured and unstressed; stressed parts may relax or crack at metallic insert interfaces.

    When Dimensional Stability at Elevated Temperature Governs Component Design

    Design calculations for load-bearing parts operating between 120 °C and 180 °C use heat-deflection temperature and coefficient of linear thermal expansion. HDT/A under ISO 75-1/2 at 1.8 MPa is typically 200–215 °C; Vicat softening temperature under ISO 306/B120 is reported between 205 °C and 215 °C. Along flow, the coefficient of linear thermal expansion is approximately 25–40 ppm/K; transverse to flow it is 60–80 ppm/K. Mold shrinkage under ISO 294-4 is anisotropic: flow-direction shrinkage 0.4–0.6% and transverse shrinkage 0.8–1.0%. Tooling calculations must apply separate flow and transverse shrinkage factors in multi-cavity layouts, especially with metal-insert overmolding.

    The high modulus of the glass-filled grade reduces creep under screw and terminal preload. Finite-element analysis should not assume isotropic properties; measured fiber orientation distributions from micro-CT or plate-section microscopy are required for accurate warpage and stress prediction. High packing pressure can create residual stress. Packing pressure of 40–60 MPa and gate-freeze time determined by sequential gate-seal studies on the production tool are recommended. Post-molding annealing at 150 °C can relieve molded-in stress but may also shift dimensions by 0.05–0.15%, so annealing must be included in tool shrinkage compensation.

    Relative to impact-modified PBT+GF30 grades, VALOX 865 prioritizes modulus and heat-deflection temperature over room-temperature notched impact. It is therefore less suitable for snap-fit designs requiring repeated strain above 1.0%, or for thin-wall covers subject to impact at -30 °C. In those applications an impact-modified PBT or unreinforced PBT should be evaluated. Relative to flame-retardant PBT-GF30 grades, VALOX 865 without flame-retardant synergists avoids halogen or phosphorus additive effects on melt stability and mold plate-out, but it cannot be used where UL 94 V-0 at 0.8 mm is a final-part requirement.

    Typical production applications include automotive engine-management housings, ignition coil bobbins, power window motor brush holders, appliance timer platforms, and lighting sockets. In terminal-receiving walls of 1.0–2.0 mm thickness, flow-direction shrinkage of 0.4–0.6% and flexural modulus near 9000 MPa allow terminal retention after thermal cycling from -40 °C to 150 °C. For parts with molded-in metal inserts, design validation should include 100–500 thermal cycles at the upper service limit because the mismatch in thermal expansion between brass or steel inserts and PBT-GF30 initiates cracking at gate-proximal weld lines. Published data for insert-specific lifetime under this exact grade is limited; tooling trials and physical aging tests on finished parts are required.

    Top