| HS Code | 231798 |
| Polymer Type | PBT |
| Glass Fiber Content | 25% |
| Flame Retardant System | Non-chlorinated/non-brominated |
| Density | 1.53 g/cm³ |
| Tensile Modulus | 9500 MPa |
| Tensile Strength | 120 MPa |
| Elongation At Break | 2.0% |
| Flexural Modulus | 9000 MPa |
| Flexural Strength | 180 MPa |
| Notched Izod Impact | 70 J/m |
| Hdt 1 82 Mpa | 195 °C |
| Hdt 0 45 Mpa | 210 °C |
| Ul94 Flame Rating | V-0 at 0.8 mm |
| Comparative Tracking Index | 400 V |
| Volume Resistivity | 1E15 ohm·cm |
| Dielectric Strength | 20 kV/mm |
| Mold Shrinkage Flow | 0.2–0.4% |
As an accredited SABIC VALOX™ PBT+GF25% Non-Cl/Br FR ENH4550 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | SABIC VALOX™ PBT+GF25% Non-Cl/Br FR ENH4550 is supplied in 25 kg moisture-barrier bags, 40 bags (1,000 kg) per pallet. |
| Container Loading (20′ FCL) | SABIC VALOX™ PBT+GF25% Non-Cl/Br FR ENH4550, packed in 25 kg bags, palletized and loaded into a 20′ FCL container. |
| Shipping | Shipping description: SABIC VALOX™ PBT+GF25% Non-Cl/Br FR ENH4550 is supplied as non-hazardous polymer pellets in sealed, moisture-barrier bags or containers. It is generally not regulated for transport under DOT/IMDG/IATA. Keep dry, protect from heat, sunlight, and contamination, and handle according to the SDS and local regulations. |
| Storage | Store SABIC VALOX™ PBT+GF25% Non-Cl/Br FR ENH4550 in a cool, dry, well-ventilated area away from direct sunlight, heat, ignition sources, and moisture. Keep in sealed original packaging, prevent contamination, and follow first-in/first-out stock rotation. Refer to the SDS for specific temperature and handling recommendations. |
| Shelf Life | Typically 24 months in original unopened packaging, stored dry at 10–30°C, protected from moisture, heat, and direct sunlight. |
Moulded case circuit breaker and miniature circuit breaker internal insulation parts are specified in SABIC VALOX™ ENH4550 where non-halogen flame retardance is required to reduce smoke corrosivity during arc faults. The 25 wt% glass fibre reinforcement lowers anisotropic shrinkage relative to unfilled PBT, which allows flat mating surfaces on line/load terminal barriers to remain within tolerance after ejection. The non-chlorinated/non-brominated FR package avoids the antimony trioxide synergist common in brominated PBT systems, therefore the melt exhibits a narrower thermal processing window than halogenated equivalents. Drying is mandatory at 120 °C for 4 h to a residual moisture level below 0.02%, because hydrolysis of the PBT matrix accelerates above 270 °C. Injection moulding should be run with a melt temperature of 250–270 °C, a mould temperature of 80–100 °C, and hold pressures sufficient to pack arc barrier ribs without overpacking the gate vestige. Total barrel residence time should remain below 5 min, and shutdown purges should use a low-MFI PBT or PC-based purging compound. Moulded arc chamber sidewalls and contact supports are then subjected to IEC 60947-2 dielectric verification and UL 94 vertical burn testing at 0.8 mm wall thickness. Published data for this specific configuration is limited; final approval requires the UL Yellow Card and supplier test report for the exact colour and thickness.
Photovoltaic junction box internal brackets and diode carrier plates are often moulded from ENH4550 when the enclosure itself is specified as UL 94 V-0 and the internal live-part insulator must satisfy IEC 62790 and UL 6703 requirements. The 25 wt% chopped glass reinforcement provides the low warpage needed for automated pick-and-place assembly of diode carriers onto printed circuit boards. Moulding uses pre-dried granulate at 120 °C for 4 h and a mould temperature at the upper end of 80–100 °C to promote crystallization and stabilise post-mould dimensions. Gate placement is critical because diode carrier bosses create multiple weld lines; a valve-gated hot runner system with sequential opening is preferred over cold sprue drops. Regrind at 15 wt% may be reincorporated only if it is kept dry, dust-free, and free of UV-stabiliser carryover from other resins. Outdoor exposure of this PBT matrix is limited; the part surface should be shielded from direct UV radiation or the housing should use an opaque cover. Terminal components include junction box main body frames, terminal clamps, and diode holder trays, each requiring glow-wire ignitability verification according to IEC 60695-2-13 at the final wall thickness.
In AC and DC electric vehicle charging couplers, ENH4550 is used for the contact insulator carrier, the locking sleeve, and the terminal retainer where IEC 62196-1 and UL 2251 define insulation coordination for pollution degree 3 conditions. The non-halogen FR system reduces corrosive gas release if the coupler is exposed to an electrical overcurrent event inside the handle. Because the contact carrier has a long flow length with local wall thickness transitions from 0.8 mm to 2.5 mm, gate position must be moved away from the contact retention slots to avoid weld line weakness. A sequential valve gate system with two or three drops is recommended for multi-contact carriers, and the hot runner manifold should be designed for balanced shear rates below the level that degrades the phosphorus-based FR. Melt temperature must not exceed 270 °C; short-term excursions above 300 °C cause FR decomposition, surface splay, and dielectric breakdown strength loss. Mould temperature is maintained at 90–100 °C to minimise post-mould shrinkage variation in the locking sleeve snap-fit. Moulded parts are tested for creepage distance retention after thermal cycling and dielectric withstand per IEC 62196-1, and comparative tracking index is evaluated according to IEC 60112. Any material lot exhibiting CTI below the value shown on the UL Yellow Card should not be used for live-part spacing without increased creepage allowances.
High-density terminal block arrays moulded in ENH4550 require stable hole-to-hole pitch retention across 12 to 24 cavities. The 25 wt% glass fibre reinforcement reduces mould shrinkage anisotropy to roughly 0.3–0.5% flow direction and 0.6–0.9% transverse direction, depending on gate location and mould temperature. Compliance is evaluated under IEC 60947-7-1 and UL 1059 for terminal block assemblies, including pull-out force, torque resistance, and dielectric withstand at rated impulse voltage. Moulding uses a stack mould with conformal cooling and a hot runner system to maintain uniform melt temperature across all cavities. Weld lines formed at metal insertion pins reduce torque resistance; the gate should be placed so that the weld line shifts to a low-stress area or an overflow well should be machined adjacent to the pin. Regrind from sprues and runners can be added at 20 wt% for non-appearance terminal bodies after re-drying, provided the regrind contains no plating contamination. Terminal products include screw-clamp terminal bodies, spring-cage terminal housings, and relay sockets requiring UL 94 V-0 at 0.8 mm.
| Test property | Standard | Application threshold |
|---|---|---|
| Flammability classification | UL 94 | V-0 at 0.8 mm wall thickness |
| Comparative tracking index | IEC 60112 | Material group IIIa/IIIb under IEC 60664-1 |
| Glow-wire ignitability | IEC 60695-2-13 | GWIT at final part thickness as specified |
| Dielectric strength | IEC 60243-1 | Verified against UL Yellow Card value |
| Water absorption | ISO 62 | ≤ 0.2% after 24 h at 23 °C |
| Density | ISO 1183-1 | 1.45 g/cm³ nominal |
Arc chamber sidewalls in miniature and moulded case circuit breakers are subjected to repeated hot-gas impingement and metallic particle deposition from contact wear. ENH4550 is evaluated for this use because its non-halogen FR package does not rely on brominated species that can form conductive char under high arc energy. The glass reinforcement level of 25 wt% reduces erosion and maintains sidewall geometry after repeated short-circuit interruptions, but the surface must be free of glass-rich skins that can reduce tracking resistance. Moulding is performed with fast injection speeds to avoid exposed fibres at the flow front and with mould temperatures of 90–100 °C to develop a resin-rich surface layer. After moulding, parts are conditioned at 23 °C and 50% RH for 48 h before IEC 60112 tracking tests; values in the 250–400 V range are typical for non-halogen glass-filled PBT grades, but the exact ENH4550 value must be taken from the UL Yellow Card and the supplier batch certificate. Thermal ageing validation follows IEC 60085 and UL 746B RTI procedures; a published RTI electrical value for this specific configuration is limited, so long-term service at continuous temperatures above 130 °C requires a dedicated EIS test. Terminal products include arc chamber sidewalls, arc dividers, and contact support floors that maintain creepage distances after specified endurance cycles in IEC 60947-2.
Solenoid coil bobbins and actuator coil formers are moulded from ENH4550 when the insulation system must pass UL 1446 winding wire compatibility testing and the bobbin flange must remain flat after coil winding. Regrind from sprues, runners, and rejected bobbins can be reincorporated at 30 wt% provided the regrind is re-dried at 120 °C for 4 h to below 0.02% moisture and is not contaminated with mould release oils or copper dust. At 30% regrind, the tensile strength and notched impact strength may decline relative to virgin material, while the UL 94 V-0 rating at 0.8 mm must be re-confirmed on the actual regrind blend and colour. The non-halogen FR package is more sensitive to repeated heat history than brominated PBT, so the number of regrind cycles should not exceed two. Moulding uses a melt temperature of 250–265 °C, a mould temperature of 80–90 °C, and a screw back pressure below 0.5 MPa to limit shear heating. Terminal products include solenoid bobbins for hydraulic valves, relay coil formers, and actuator winding carriers tested per IEC 61858 or UL 1446.
Competitive SABIC VALOX™ PBT+GF25% Non-Cl/Br FR ENH4550 prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
SABIC VALOX™ PBT+GF25% Non-Cl/Br FR ENH4550 is a non-brominated, non-chlorinated flame-retardant polybutylene terephthalate compound reinforced with 25% glass fibre. The grade is supplied as injection-moulding pellets and is specified where UL 94 V-0 performance is required without halogenated flame-retardant chemistry. Published datasheet values place the nominal density at 1.60 g/cm³ under ISO 1183-1 and the nominal flexural modulus at 8000 MPa under ISO 178. The material is used in low-voltage electrical and electronic components where dimensional stability, chemical resistance, and high comparative tracking index are required. Typical applications include connectors, relay housings, switch components, circuit-breaker internal parts, and photovoltaic junction enclosures. Table 1 consolidates the nominal published values; these values are not specification limits and must be confirmed against the current manufacturer technical datasheet before tool design.
| Property | Test method | Nominal value |
|---|---|---|
| Glass fibre content | ISO 3451-1 | 25 % |
| Density | ISO 1183-1 | 1.60 g/cm³ |
| Melt volume-flow rate | ISO 1133-1 at 250°C/5.0 kg | 18 cm³/10 min |
| Tensile stress at break | ISO 527-2/5 | 105 MPa |
| Tensile strain at break | ISO 527-2/5 | 2.2 % |
| Flexural modulus | ISO 178 | 8000 MPa |
| Notched Izod impact strength, 23°C | ISO 180/1A | 5 kJ/m² |
| Heat deflection temperature, 1.80 MPa | ISO 75-2/Ae | 190°C |
| Vicat softening temperature, B120 | ISO 306 | 205°C |
| Comparative tracking index | IEC 60112 | 600 V |
| Dielectric strength | IEC 60243-1 | 17 kV/mm |
| Volume resistivity | IEC 60093 | 1.0E+15 ohm·cm |
| Flammability classification | UL 94 | V-0 at 0.75 mm |
| Flammability classification | UL 94 | 5VA at 2.5 mm |
Comparative tracking index is a discriminating variable. The ENH4550 datasheet reports a nominal CTI of 600 V under IEC 60112, which is desirable for creepage paths in connectors operating at mains voltage. Brominated PBT systems based on antimony trioxide synergist may exhibit lower CTI values because the antimony oxide phase participates in transient surface conduction at arcing temperatures. The absence of brominated aromatic compounds also removes the potential for hydrogen bromide evolution during thermal degradation; however, the phosphorus-dominated char mechanism replaces the gas-phase radical quenching of brominated systems with condensed-phase barrier formation. This shift in mechanism explains the need to verify glow-wire ignition temperature under IEC 60695-2-12 and tracking resistance under IEC 60112 using the specific wall thickness of the moulded article rather than converting from brominated-grade data. Smoke density under ISO 5659-2 is not a standard datasheet property for moulding compounds, and comparative values between ENH4550 and brominated PBT at identical glass loading are not routinely published. However, the elimination of brominated aromatic compounds removes the primary source of corrosive hydrogen bromide during incomplete combustion. Combustion gas composition should still be verified by DIN EN 45545-2 when railway interior applications are specified, because glass-filled PBT may release carbon monoxide and particulate soot regardless of flame-retardant chemistry.
For production-scale injection moulding, desiccant drying at 120°C for 3 h to 4 h to a residual moisture level below 0.02% is mandatory. Hydrolysis of polybutylene terephthalate proceeds rapidly above the melt processing temperature when moisture is present; a dew-point meter at the dryer air inlet with a reading of -30°C or lower is recommended. If incoming granulate has been exposed to open air at 23°C and 50% RH for more than 1 h, verification by Karl Fischer titration per ISO 15512 is advised before processing. A general-purpose screw with an L/D ratio of 20:1 to 25:1, a compression ratio of 2.5:1, and a free-flow non-return valve is appropriate. Back pressure should be maintained between 0.3 MPa and 0.5 MPa to ensure homogeneous glass distribution without excessive shear heating. Melt temperature measured at the nozzle should be kept within 250°C to 270°C; mould temperature should be controlled between 60°C and 100°C to promote crystallisation and achieve consistent shrinkage. At the upper mould temperature boundary, ejection forces may increase if undercuts or textured surfaces are not drafted beyond 1° per side. Shot size should occupy 30% to 70% of barrel capacity to limit residence time, and cushion should be maintained between 3 mm and 6 mm. For a typical connector with projected area of 100 cm², a cavity pressure of 40 MPa corresponds to a clamp force requirement of 400 kN; actual clamp force must be calculated from cavity-pressure simulation and part geometry.
Fill pressure in thin-wall tools is governed by melt volume-flow rate and solidification rate. The nominal MVR for ENH4550 at 250°C and 5.0 kg load is published in the product datasheet; it should be used with pressure-drop simulation rather than as a single indicator of mouldability. Pressure-driven jetting can occur when gate diameters are below 0.8 mm and wall thicknesses are below 0.75 mm. Direct edge gates or fan gates with a land length of 0.5 mm to 1.0 mm are preferred; tunnelled sub-gates should be designed with a minimum included angle of 45° and a gate diameter not less than 0.8 mm. In multi-cavity tools, flow balancing must be verified by short-shot analysis, because glass-fibre orientation distribution changes with flow length and can shift shrinkage anisotropy from 0.3% to 0.6% in the flow direction. Hot-runner manifolds with internal needle-valve nozzles must be configured to avoid dead spots; the maximum melt residence time at 260°C should not exceed 5 min. At higher residence times, surface streaking and gas jets at the gate may be observed, consistent with incipient degradation of the non-halogen flame-retardant package.
Tool-filling simulations require shear-rate-dependent viscosity measured by capillary rheometry rather than MVR alone. The grade exhibits pseudoplastic behaviour typical of glass-filled PBT; the power-law consistency index and flow index should be obtained from a capillary rheometer using a die length-to-diameter ratio of 20:1 at 260°C. Simulation input should include glass-fibre orientation from processing conditions, because tensile modulus in the flow direction may exceed cross-flow modulus by 20% to 40%; published data for this specific configuration is limited and should be generated for critical load-bearing bosses. Weld lines in glass-reinforced PBT can reduce tensile strength by 30% to 50% relative to unwelded sections under ISO 527-2. Gate placement must position weld lines away from snap-fit latches or thin membrane regions. Multiple hot tips increase weld-line count and should be avoided unless flow simulation demonstrates acceptable pressure drop and mechanical test coupons confirm weld-line strength.
Connector housings for photovoltaic junction boxes expose the polymer to direct sunlight, thermal cycling, and potential partial discharge. The material’s HDT/Af of 190°C under ISO 75-2/Ae supports short-term thermal excursions during soldering; however, long-term UV ageing and hydrolysis resistance in the specific junction-box construction are not fully described by standard datasheet properties. Users must evaluate the grade under UL 746C f1 outdoor suitability criteria if the application is exposed to UV and water immersion. Relay bases and contact carriers benefit from the nominal CTI of 600 V under IEC 60112, but the design must separate high-current terminals by creepage distances calculated according to IEC 60664-1 for the actual pollution degree environment. For press-fit pins inserted into printed circuit boards, room-temperature notched Izod impact strength of 5 kJ/m² under ISO 180/1A does not predict pinned-hole cracking resistance after ageing at 85°C. Application-specific thermal cycling with strain-gauge instrumented holes is required for reliability assessment.
Because the grade is marketed as non-chlorinated and non-brominated, verification is typically performed by oxygen bomb combustion followed by ion chromatography per EN 14582. The interpretation of halogen-free depends on the maximum allowable chloride and bromide content in the relevant industry specification. For printed circuit board laminates, IEC 61249-2-21 defines a maximum of 900 ppm total chlorine and 900 ppm total bromine, but the same numerical limits are not automatically applicable to moulded plastics unless the customer specification adopts them. The grade is suitable for RoHS recast compliance assessment under Directive 2011/65/EU as amended by (EU) 2015/863 at the homogeneous-material level, but the final article must still be assessed for other restricted substances such as lead, mercury, cadmium, and specific phthalates. REACH SVHC screening should be completed by the downstream supplier because the compound supplier cannot report against every formulation-specific impurity. Table 2 lists the principal compliance instruments applicable to this product class.
| Regulation / standard | Applicability | Assessment method |
|---|---|---|
| Directive 2011/65/EU and (EU) 2015/863 | RoHS substance restrictions in homogeneous materials | XRF screening plus GC-MS / ICP-OES |
| REACH Regulation (EC) No 1907/2006 | SVHC disclosure | SCIP database / supplier confirmation |
| IEC 61249-2-21 | Halogen-free definition for laminates; customer-specific adaptation for plastics | EN 14582 oxygen bomb combustion |
| UL 94 | Flammability classification | UL Yellow Card |
| IEC 60112 | Tracking resistance | Tracking index test |
| UL 746C | Outdoor suitability | f1 / f2 rating application-specific |
Compared with a brominated PBT GF25 product, the ENH4550 formulation replaces the brominated resin and antimony trioxide carrier with a phosphorus-based flame-retardant system. Antimony trioxide has a theoretical density of 5.7 g/cm³; its removal lowers formulation density and can reduce part weight at equivalent glass loading. The condensed-phase char former can also increase melt viscosity at low shear rates, which may require higher melt temperature or reduced regrind levels. Published data on the specific effect of regrind incorporation on UL 94 performance for ENH4550 is limited; therefore, production moulders should limit regrind to 20% by weight unless validation trials demonstrate unchanged flammability, CTI, and mechanical properties. The material should not be blended with brominated PBT compounds, because mixed flame-retardant mechanisms do not necessarily combine additively and may reduce tracking resistance or cause plate-out. Similarly, addition of amine-based nucleating agents or mould-release concentrates should be avoided unless compatibility with the phosphorus flame retardant is confirmed in advance, because interactions can alter crystallisation rate and shift part dimensions.
Compared with non-FR 25% glass-filled PBT, ENH4550 carries a flame-retardant package that increases melt viscosity and may reduce tensile strain at break. The nominal tensile strain at break of 2.2% indicates a stiff, low-ductility material. Snap-fit designs with high strain should be prototyped using production-like cooling rates because rapid quench in thin walls may reduce crystallinity and alter yield strain relative to laboratory specimen data. Glass-fibre orientation near the surface freezes under high shear, while the core orientation may differ; differential shrinkage between flow and transverse directions can produce warpage in flat parts exceeding 0.1 mm per 25 mm of length. Mould temperature uniformity of ±2°C is required to avoid plate curvature. Post-mould dimensional inspection should be performed after conditioning at 23°C and 50% RH for 48 h under ISO 291. For components with metal inserts, processing trials must measure hoop stress and insert-to-polymer adhesion, because the high glass loading and low elongation at break limit stress relaxation at the interface. The material is not recommended for direct food-contact use unless the final article meets applicable food-contact requirements; published data for this specific configuration is limited.