Sabic Valox Pbt Gf20 Super Hf Shf4340

SABIC VALOX™ PBT+GF20%-Super-HF SHF4340

    • Product Name: SABIC VALOX™ PBT+GF20%-Super-HF SHF4340
    • Factroy Site: Yinchuan, Ningxia, China
    • Price Inquiry: sales8@ascent-chem.com
    • Manufacturer: Ascent Petrochem Holdings Co., Limited
    • CONTACT NOW
    VTB
    Specifications
    HS Code 678512
    Polymer Base PBT
    Glass Fiber Content 20% by weight
    Density 1.45 g/cm³
    Tensile Modulus 7,000 MPa
    Tensile Strength At Break 100 MPa
    Elongation At Break 2.5%
    Flexural Modulus 6,500 MPa
    Flexural Strength 150 MPa
    Notched Izod Impact At 23 C 5 kJ/m²
    Heat Deflection Temperature At 0 45 Mpa 220 °C
    Heat Deflection Temperature At 1 8 Mpa 200 °C
    Vicat Softening Temperature 210 °C
    Melting Temperature 225 °C
    Mold Shrinkage Flow Direction 0.3–0.6%
    Water Absorption 24h 0.06%
    Ul 94 Flame Rating HB

    As an accredited SABIC VALOX™ PBT+GF20%-Super-HF SHF4340 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.

    Packing & Storage
    Packing SABIC VALOX™ PBT+GF20%-Super-HF SHF4340 is supplied in 25 kg moisture-barrier bags, palletized for industrial shipping and storage.
    Container Loading (20′ FCL) 20′ FCL container loading for SABIC VALOX™ PBT+GF20%-Super-HF SHF4340: 25 kg bags on pallets, evenly distributed, dry, stable, secure stowage.
    Shipping SABIC VALOX™ PBT+GF20%-Super-HF SHF4340 is shipped as non-hazardous thermoplastic resin pellets in moisture-barrier bags, sacks, or octabins. No UN number or dangerous-goods class applies. Store in a cool, dry area and protect from direct sunlight, heat, and moisture; follow local transport regulations.
    Storage Store SABIC VALOX™ PBT+GF20%-Super-HF SHF4340 in a cool, dry, well-ventilated area, away from direct sunlight, heat sources, moisture, and strong odors. Keep original bags or containers tightly closed to prevent contamination, dust, and static buildup. Maintain dry conditions; follow supplier-recommended drying before processing. Use first-in, first-out rotation and observe the indicated shelf life. Avoid excessive stacking or package damage.
    Shelf Life Shelf life is typically 24 months in original, unopened packaging stored dry below 30°C, protected from moisture and contamination.
    Application of SABIC VALOX™ PBT+GF20%-Super-HF SHF4340

    Powertrain and chassis wiring harness connectors moulded in VALOX™ PBT+GF20%-Super-HF SHF4340 typically fail not from short-term heat ageing but from loss of terminal latch retention after repeated service actions. In sealed low-voltage connector housings with 1.2 mm terminal pitch, the minimum latch-beam wall often falls to 0.40–0.50 mm, and the high-flow PBT matrix permits cavity filling at injection speeds of 180–250 mm/s without exceeding 140 MPa hydraulic peak pressure in a 32-cavity tool. Pre-drying at 120 °C for 4 h in a dry-air dryer with dew point ≤ -30 °C is required; residual moisture above 0.02 % by ISO 15512 initiates hydrolysis during plastication and yields brittle failure at terminal insertion. Barrel settings from feed throat to nozzle are maintained at 230 °C, 240 °C, 250 °C, 250 °C, 250 °C, with actual melt temperature measured at 245–260 °C and mould temperature held at 80–90 °C to promote crystallinity. The 20 wt% glass-fibre loading dictates anisotropic post-mould shrinkage: representative flow-direction shrinkage is 0.35–0.50 % and transverse shrinkage 0.65–0.90 % when measured on 60 mm × 60 mm × 2 mm plaques per ISO 294-4; multi-cavity layouts are compensated by iterative steel adjustments. Regrind addition from cold-runner scrap is limited to ≤ 15 wt% because repeated extrusion reduces fibre length and notched impact strength under ISO 179-1/1eA. Electrical connector validation follows SAE/USCAR-2 for terminal retention, water intrusion, and thermal cycling, while material mechanical conformance is recorded by ISO 527-2/1A and ISO 178. The terminal product is the engine-compartment sealed connector used in low-voltage sensor and actuator harnesses; flame retardance to UL 94 V-0 is not provided by this non-FR grade and must be addressed by selecting a flame-retarded VALOX variant if the connector is located near high-current busbars.

    What Causes Winding Creep in Relay Coil Formers at 120 °C?

    Relay coil formers wound with enamelled copper magnet wire impose a sustained hoop stress on the flanges of a bobbin at operating temperatures that can reach 120 °C in industrial control panels. The relevant failure is not immediate fracture but progressive flange distortion that closes the armature air gap and shifts the relay pull-in voltage beyond the IEC 61810-1 electromechanical relay tolerance. VALOX SHF4340 moulded with a single edge gate at the flange perimeter orients the glass fibres circumferentially and reduces anisotropic creep, whereas two opposing gates place a weld line through the flange and degrade creep cracking resistance. Tensile creep modulus measured under ISO 899-1 at 120 °C after 1,000 h falls below the initial modulus; comparative GF20 PBT compounds can retain 50–60 % of initial modulus depending on mould-induced crystallinity, though published creep data specific to SHF4340 is limited. Mould temperature below 60 °C produces underdeveloped crystalline structure and accelerates creep; a mould temperature of 90–100 °C is specified for coil formers with flange thickness below 0.8 mm. Winding tension is set between 0.5 N and 1.2 N for wire diameters of 0.1–0.2 mm, and terminal pin holes are sized to produce 0.05–0.08 mm interference with brass pins. The coil former should be preheated to 85 °C before hot-staking of terminals to avoid microcracking at the pin interface. Creepage and clearance distances follow IEC 60664-1, and comparative tracking index of unmodified GF20 PBT is typically in the 250–300 V range under IEC 60112; the value for SHF4340 must be confirmed from the supplier datasheet. Terminal product is the injection-moulded coil bobbin in general-purpose power relays and contactor auxiliary relays, not high-voltage isolation relays where a flame-retarded, high-CTI grade is mandatory.

    Valve-Gate Orifice Variables and Fibre Length Retention in 64-Cavity Tools

    Running SHF4340 in a 64-cavity hot-runner tool for terminal position assurance slides shifts the limiting defect from sink marks to gate freeze and fibre attrition at the gate land. The 20 wt% glass loading is sheared when the melt passes through a valve-gate orifice below 0.8 mm; fibre length reduction of more than 40 % occurs in the gate region and lowers tensile strength in the adjacent rib by up to 20 % under ISO 527-2/1A, though published fibre-length data for SHF4340 specifically is limited. A gate land length of 0.8–1.2 mm and gate orifice diameter of 0.9–1.4 mm for 1.0–1.5 mm wall stock prevent excessive shear heating while retaining sufficient gate freeze control. Hot-runner manifold and nozzle tips are set at 250–260 °C; melt residence time in the manifold must not exceed 5 min, otherwise hydrolysis and thermal degradation produce yellowing and a measurable drop in MFR under ISO 1133-1:2022 at 250 °C/2.16 kg. Barrel shot weight is maintained at 50–80 % of capacity to minimise residence time. The table below records representative production-trial data for GF20 high-flow PBT in a 64-cavity hot-runner tool at 1.0 mm nominal wall thickness; actual values are tool-specific and require verification for SHF4340.

    Gate orifice diameterPeak fill pressureGate freeze intervalObserved defect mode
    0.6 mm135–155 MPa<0.3 sShort shot, fibre breakage
    0.9 mm100–125 MPa0.4–0.6 sAcceptable fill, minor gate vestige
    1.2 mm80–100 MPa0.8–1.1 sStable process, low shear
    1.6 mm65–80 MPa>1.2 sStringing, post-mould dimensional drift

    After ejection, ISO 294-4 shrinkage measurement on flat sections of the terminal position assurance slide shows flow-direction shrinkage 0.30–0.50 % and transverse shrinkage 0.65–0.90 %; the asymmetry requires gate positions aligned with the functional datum faces rather than the part centroid. Terminal product is the mass-produced TPA slide in multi-pin connector systems; the process data also transfers to high-cavitation fuse-box terminal carriers, provided the hot-runner balance is verified by short-shot progression.

    When cylindrical sensor bodies integrate overmoulded brass inserts, the dominant process variable is the differential thermal contraction between insert metal and the PBT matrix after ejection from the tool. In an M12×1.5 brass insert, the insert should be heated to 120 °C ± 10 °C before robot placement; insert temperature below 80 °C produces radial hoop stress in the surrounding boss that initiates stress cracking after thermal cycling between -25 °C and 100 °C. The mould temperature is set to 90 °C, and the insert is positioned with a 0.05–0.10 mm axial preload against the core to prevent melt flash into the thread. Careful gate placement is required because the melt splits around the insert and creates a weld line on the load-bearing side of the threaded boss; the gate is moved to the flange perimeter and the weld line is displaced into a non-load path. Thread engagement length is maintained at 1.5 times the thread nominal diameter to prevent boss shear before insert pull-out in end-use assembly. Torque retention is validated by a series of M12 mating fasteners at 1.5–2.5 N·m but the limiting value is geometry-specific; published torque retention data for SHF4340 with a particular knurl pattern is limited and must be established by insert supplier validation. Dimensional stability of the sensor sealing face is checked after 24 h conditioning at 23 °C/50 % RH; total flatness deviation over a 30 mm diameter sealing face is held below 0.10 mm per ISO 1101. Chemical exposure testing follows ISO 175 with typical hydraulic oil and cutting fluid environments at 85 °C for 500 h; PBT is susceptible to alkaline cutting fluids above pH 10, which causes surface etching and loss of gloss without significant section loss. Terminal product is the cylindrical inductive proximity sensor housing with overmoulded threaded insert, not the sensing face where polymer creep under constant load must be re-evaluated.

    When the Flexible Latch Beam Falls Below 0.45 mm in Power-Tool Switch Housings

    If a cordless power-tool trigger housing specifies a flexible latch beam of 0.40 mm for contact retention, the glass-fibre orientation in the beam becomes the controlling quality parameter. In sections below 0.45 mm, the 20 wt% glass reinforcement concentrates in the core and the glass-poor skin carries most tensile strain; transverse tensile strength measured on a 2 mm plaque by ISO 527-2/1A may be 30–35 % lower than flow-direction tensile strength because of fibre alignment along the flow path. For this reason the latch beam is gated directly along its length rather than filled transversely, and the injection speed is set to 180–250 mm/s to prevent freeze-off before the thin wall is complete. Hold pressure is capped at 60–80 MPa for 4–6 s; higher hold pressure above 90 MPa can overpack the gate region and crack the thin beam at ejection, particularly when the mould temperature is below 70 °C. Ejector pins are replaced by blade ejectors with 0.8–1.0 mm thickness spaced every 8–10 mm along the beam. Regrind content from this ultra-thin-wall tool is limited to ≤ 10 wt% because the high shear history shortens glass fibre length and lowers thin-section elongation at break, although published SHF4340-specific thin-wall regrind data is limited. The switch housing is tested for drop impact at -20 °C under IEC 60068-2-31 and for contact retention after 2,500 cycles of trigger travel; material tensile and impact values are recorded with ISO 527-2/1A and ISO 179-1/1eA. Terminal product is the injection-moulded trigger switch housing in brushless cordless drill and impact driver assemblies, where the flame retardance class is governed by UL 94 HB unless the end product requires a V-0 housing.

    Motorized HVAC actuator gear carriers and sector gear fatigue.

    Production of HVAC blend-door actuator gear carriers subjects SHF4340 to constant spring torque and occasional 85 °C soak in the instrument panel. The gear carrier is not a high-speed gear; failure occurs by creep of the bearing boss under a continuous 15–25 N spring load, leading to gear mesh misalignment and intermittent tooth skipping. Boss creep is measured by ISO 899-1 tensile creep after 1,000 h at 85 °C; comparative GF20 PBT and glass-reinforced acetal data show PBT retains dimensional stability at elevated temperature but has higher friction against steel shafts than acetal. For this reason the gear carrier is not run dry against a steel worm; a polyalphaolefin grease compatible with PBT is specified at 0.5–1.0 mg per bearing interface. Gate placement at the hub centre creates a weld line at the outer flange; moving the gate to the peripheral ring and using a mould temperature of 80–90 °C improves fibre orientation and delays creep. Concentricity of the bearing bore to the gear-axis datum is held within 0.05 mm total indicated runout per ISO 1101; post-mould moisture uptake below 0.1 % does not shift bore diameter beyond this tolerance. Fatigue load capacity of moulded gear elements is estimated per VDI 2736-4 where applicable, although the gear carrier itself is not a loaded gear flank and serves as structural housing. Terminal product is the automotive HVAC blend-door actuator gear carrier and sector gear support plate; direct replacement of acetal carriers should not occur without checking dimensional shrink and clearance, as published system-level validation data for SHF4340 is limited.

    Free Quote

    Competitive SABIC VALOX™ PBT+GF20%-Super-HF SHF4340 prices that fit your budget—flexible terms and customized quotes for every order.

    For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.

    We will respond to you as soon as possible.

    Tel: +8618005193850

    Email: sales8@ascent-chem.com

    Inquiry

    Get Free Quote of Ascent Petrochem Holdings Co., Limited

    Flexible payment, competitive price, premium service - Inquire now!

    Certification & Compliance
    More Introduction

    SABIC VALOX™ PBT+GF20%-Super-HF SHF4340 is a 20 wt% glass-fibre-reinforced polybutylene terephthalate injection-moulding compound in which the polymer architecture and flow-modifier package are balanced to reduce melt viscosity relative to standard PBT-GF20 at equivalent barrel set-points. The material is positioned for high-cavitation, thin-wall electrical and electronic components where the molten charge must fill gates from 0.5 mm to 1.2 mm without exceeding available injection pressure. Lot-specific physical and mechanical characterisation is reported under ISO 1183-1, ISO 527-2, ISO 178, ISO 180/1A, ISO 75-1/-2, and ISO 1133-1. The nominal glass loading is confirmed by thermogravimetric ash content according to ISO 3451-1 Method A. The Super-HF identifier is a SABIC flow-class designation and does not confer flame retardancy, ultraviolet stabilisation, or food-contact status. Primary application areas include sealed connectors, relay bases, sensor housings, camera modules, and power tool enclosures in which heat deflection, creep resistance, and moulding-dimensional repeatability are specified according to ISO 294-4 after conditioning in ISO 291 standard atmospheres.

    The property envelope in the table below is a reference band for 20 wt% glass-fibre-reinforced PBT grades with super-high-flow modification. It is not a substitute for the SABIC lot certificate, and production design values must be confirmed against the current supplier datasheet.

    PropertyTest methodSHF4340 reference envelopeStandard PBT+GF20 envelopeUnfilled PBT envelope
    DensityISO 1183-11.45–1.50 g/cm³1.45–1.52 g/cm³1.30–1.32 g/cm³
    Tensile modulusISO 527-26000–8000 MPa6500–8500 MPa2500–2800 MPa
    Tensile stress at breakISO 527-290–110 MPa100–120 MPa50–60 MPa
    Flexural modulusISO 1785500–7000 MPa6000–8000 MPa2000–2400 MPa
    Notched Izod impact at 23 °CISO 180/1A4–7 kJ/m²5–8 kJ/m²3–5 kJ/m²
    Heat deflection temperature, method A, 1.8 MPaISO 75-1/-2195–210 °C200–215 °C50–60 °C
    Melt volume-flow rate at 250 °C/2.16 kgISO 1133-125–45 cm³/10 min15–25 cm³/10 min15–40 cm³/10 min

    Which Drying and Injection Parameters Govern Thin-Wall Moulding?

    Residual moisture must be held below 0.02% before plastication because PBT undergoes hydrolytic chain scission when moisture is carried into the melt. The compound is normally dried in a desiccant dryer with a dew point of ≤ -40 °C at 120 °C for 3 h to 4 h. Moisture determination after drying is performed by ISO 15512 Method B using coulometric Karl Fischer titration. Drying conditions are not discretionary for thin-wall tools: inadequate drying produces splay, brittle snap-fit failure, and lot-to-lot dimensional drift.

    Processing parameterStarting rangeMeasurement or control basis
    Predrying temperature120 °CDesiccant dryer hopper thermocouple
    Predrying time3–4 hDryer residence timer
    Residual moisture after drying≤ 0.02%ISO 15512 Method B
    Melt temperature245–270 °CBarrel zone set-points with melt probe verification
    Mould temperature40–80 °CMould surface thermocouple per ISO 294-4
    Injection velocity50–150 mm/sScrew position transducer and filling-time recorder
    Back pressure0.3–0.7 MPaHydraulic pressure gauge or machine transducer
    Hold pressure50–80 MPaNozzle or cavity pressure sensor
    Residence time at 260 °C< 4 minShot weight, cycle time, and barrel capacity calculation

    On high-cavitation tools the limiting factor is usually barrel residence time rather than melt temperature. Holding the melt at 260 °C for more than 4 min can shift molecular weight distribution and reduce weld-line strength. The effect may be detected as a drop in melt viscosity during purge, visible yellowing, or an increase in low-molecular-weight volatiles. Screw recovery time should be kept short, and shot mass should be sized between 25% and 75% of barrel capacity to avoid excessive thermal history.

    Within sealed automotive connector bodies and sensor housings, the grade is used when internal ribs, bosses, and snap-fit features require molten material to fill opposing walls without hesitation marks or pressure-limited short shots. Dimensional stability is evaluated after 48 h at 23 °C/50% RH using shrinkage measurements derived from cavity-to-moulding comparisons under ISO 294-4. The compound is not marketed as a flame-retardant grade; the current UL 94 classification must be checked against the SABIC yellow card for the moulded wall thickness being used. Applications requiring V-0 performance at 0.8 mm or 1.5 mm should be directed to flame-retardant PBT grades rather than relying on Super-HF flow modification.

    Flow-Length and Weld-Line Strength Trade-Offs in 20%-Glass-Fibre PBT

    Compared with a standard PBT-GF20 grade, SHF4340 changes the processing-vs-toughness balance. The polymer fraction is formulated to sustain higher melt volume-flow rate under ISO 1133-1 at 250 °C/2.16 kg, which shortens filling time in multi-cavity tools. The glass-fibre content remains 20 wt% by ash content per ISO 3451-1, so short-term tensile modulus remains in the same class as standard PBT-GF20. Weld-line strength, however, is not governed solely by fibre fraction; it depends on flow-front temperature, fibre orientation at the meeting plane, and the angle of merging fronts. When two advancing fronts meet at an angle below 75°, the weld line in high-flow PBT can retain less elongation than a standard PBT-GF20 because lower melt viscosity permits a thinner frozen skin and different orientation distribution near the weld plane. Published data for this specific configuration is limited, so tool-specific weld-line tensile specimens cut from the gate region and weld region and tested under ISO 527-2 are required for confirmation.

    The grade does not alter the inherent chemical resistance of PBT to aliphatic hydrocarbons, lubricating greases, or mild brake fluids at room temperature. However, it is not a replacement for hydrolytically stabilised PBT or polyphenylene sulphide in hot-water/glycol systems above 100 °C. The main formulation trade-off is that the flow improvement package can reduce low-temperature impact response relative to a toughened PBT grade. Notched Izod values at -30 °C under ISO 180/1A should be treated as a design limit rather than an afterthought, particularly for snap-fits that operate under impact loading in outdoor equipment.

    When Hot-Runner Manifolds Extend Residence Time Past 4 Minutes

    Hot-runner systems introduce additional thermal duty that must be evaluated before the grade is released for production. A manifold temperature above 270 °C or a hot-drop idle period longer than 4 min can degrade the flow-modifier package and create inconsistent filling between cavities. Manifold zone set-points should be profiled so that the melt experiences no more than 5 °C excursion above the rear-zone barrel set-point. If sequential valve gating is used, cavity-fill imbalance is diagnosed by short-shot series and part-mass stability studies rather than by visual inspection alone.

    Regrind from sprues, runners, and rejected parts may be re-introduced only after verification of glass-fibre length retention. Multiple heat histories reduce fibre length and lower notched impact even when the pelletised regrind fraction remains below 20 wt%. The acceptable regrind level must be confirmed on the production tool by testing notched Izod specimens under ISO 180/1A and tensile specimens under ISO 527-2 from moulded parts containing the intended regrind ratio. Avoid combining the melt with amine-based colour concentrates or additives because PBT is susceptible to aminolysis, which can cause molecular weight reduction and surface bloom.

    Top