| HS Code | 960509 |
| Polymer | Polybutylene terephthalate (PBT) |
| Filler | 30% glass fiber |
| Color | Black |
| Flame Retardant | Yes |
| Density | 1.53 g/cm³ |
| Tensile Modulus | 10000 MPa |
| Tensile Stress At Break | 120 MPa |
| Tensile Strain At Break | 2.0% |
| Flexural Modulus | 9000 MPa |
| Flexural Strength | 170 MPa |
| Notched Izod Impact Strength At 23 C | 8 kJ/m² |
| Hdt At 1 8 Mpa | 200°C |
| Hdt At 0 45 Mpa | 215°C |
| Ul94 Flammability Rating | V-0 at 0.75 mm |
| Water Absorption | 0.1% |
| Melt Volume Rate At 250 C 5 Kg | 8 cm³/10 min |
| Mold Shrinkage Flow | 0.3-0.5% |
| Processing Melt Temperature | 240-260°C |
| Mold Temperature | 60-90°C |
| Drying Temperature | 120°C |
| Drying Time | 4 h |
As an accredited SABIC VALOX™ PBT-FR 420SE0-BK1066 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | SABIC VALOX™ PBT-FR 420SE0-BK1066 is supplied in 25 kg moisture-proof bags, securely sealed and labeled for industrial handling. |
| Container Loading (20′ FCL) | Loading of SABIC VALOX™ PBT-FR 420SE0-BK1066 into a 20-foot FCL container, palletized and secured for export shipment. |
| Shipping | SABIC VALOX™ PBT-FR 420SE0-BK1066 is supplied as black flame-retardant PBT resin pellets in sealed, moisture-barrier bags or boxes. It is generally non-hazardous for transport and not classified as dangerous goods. Keep dry, avoid heat/contamination, store in a cool, dry area, and follow the SDS and local shipping regulations. |
| Storage | Store SABIC VALOX™ PBT-FR 420SE0-BK1066 in a cool, dry, well-ventilated area away from direct sunlight, heat, flames, and ignition sources. Keep containers tightly closed to prevent moisture pickup and contamination, and separate from strong oxidizing agents. Use appropriate secondary containment and follow the manufacturer’s SDS and local regulations for safe storage and handling. |
| Shelf Life | SABIC VALOX™ PBT-FR 420SE0-BK1066 has a typical shelf life of 24 months when stored dry, cool, and in original sealed packaging. |
Processing of 30 wt% glass-fiber flame-retardant PBT in low-voltage distribution equipment begins with the recognition that IEC 60664-1:2020 insulation coordination and IEC 60947-1 low-voltage switchgear verification address the molded part, not the resin pellet. The compound is introduced at 100 wt% as supplied; sprue and runner regrind from the same black lot is limited to 15 wt% of total shot mass because higher regrind fractions can reduce melt-bank homogeneity and create local flame-retardant dilution at knit lines around cage-clamp terminal apertures. Drying is mandatory at 120 °C for 4 h in a desiccant dryer with a dew point of −40 °C or lower until ISO 15512:2019 or ASTM D6980-17 moisture measurement is below 0.02%; if plant relative humidity exceeds 60%, open-hopper residence time after drying is kept below 20 min and the loader circuit is closed-loop dry air. Barrel setpoints from rear zone to nozzle are 240–250 °C rear, 250–260 °C center, 255–265 °C front, and 260–265 °C nozzle; screw L/D of 20:1 to 25:1 with compression ratio 2.0:1 to 2.5:1 prevents excessive shear heating that decomposes the flame-retardant package. Mold temperature is held at 80–100 °C to reduce differential fiber orientation between hot gate regions and cold flow-front regions. Gate location is placed to move weld lines away from terminal retention springs; venting depth is maintained at 0.01–0.02 mm because flame-retardant volatiles produce gas burns at inadequate vent depth. The resulting articles include miniature circuit breaker covers, busbar supports, and cage-clamp terminal housings with nominal wall thickness at or above 1.5 mm, where UL 94 V-0 is assessed on the end-use molded part rather than inferred from pellet-level data.
The underhood connector segment imposes a different set of failure modes: terminal retention loss after vibration, stress cracking at brass insertion points, and surface bloom after exposure to hot windshield washer fluid. Compliance is normally based on SAE/USCAR-2 Rev 7 performance testing and, for German programmes, LV214-1; the material is not an autonomous approval because the connector cavity design, terminal lance, and seal interface all participate in the test outcome. In this application the rigid shell is molded from 100 wt% of the supplied compound; the addition ratio is not reduced by the overmolded TPE wire-entry seal, because the seal is a second component and does not dilute the PBT phase. Regrind from sprues and short shots is capped at 10 wt% of total shot mass when the molded part must survive 1000 h of ISO 16750-4 high-temperature exposure plus vibration. Drying uses 120 °C for 4 h to 0.02% moisture; the machine is configured with a general-purpose glass-filled polyester screw, L/D 20:1, back pressure 0.3–0.7 MPa, and mold temperature 70–90 °C. For insert molding of brass terminals, inserts are preheated to 80–100 °C before insertion to reduce localized cooling and internal tensile stress at the pin base; mold filling uses a fill speed that produces 1–2 s fill time for typical multi-cavity connector tools, with holding pressure falling by 50–70% from peak injection pressure and screw decompression 2–3 mm before retract to prevent nozzle drool. The resulting parts are engine control unit connectors, body control module connector bodies, and transmission speed sensor housings.
For household appliance power modules, the missing variable in most qualification plans is not flame retardance but glow-wire end-product classification under IEC 60335-1 Clause 30.2.3.1 and IEC 60695-2-11, because unattended appliances with current-carrying connections above 0.2 A must be tested as complete parts, not inferred from a resin UL 94 yellow card. The compound is processed at 100 wt% of the polymer matrix; adding a halogen-free flame-retardant masterbatch to adjust glow-wire performance is not recommended because the existing flame-retardant system is fixed and dilution shifts the ignition temperature in an uncontrolled manner. A maximum of 20 wt% in-house regrind from identical lot sprues and runners is permissible only if the regrind is dried to 0.02% and final glow-wire tests are repeated on the actual black molded part. Molding uses barrel settings from 245 °C rear to 260 °C nozzle, mold temperature 80 °C, and screw cushion 3–5 mm; for a large flat control module frame, sequential valve gating is used to move the flow front linearly and avoid center-knit warp. Vent depths are held at 0.01–0.02 mm and the screw is a low-to-medium compression glass-reinforced polyester design to avoid excess shear heating. Amine-based processing aids are avoided because they can accelerate ester cleavage at melt temperature and lower melt viscosity during residence time. The resulting components are dishwasher power control module frames, washing machine motor control housings, and refrigerator inverter control boxes, all of which require post-mold dimensional checks under ISO 294-4 for shrinkage consistency.
For EV couplers and on-board charger housings, wall sections of 0.8–1.5 mm are common, and the standards IEC 61851-1, IEC 62196-2, UL 2251, and SAE J1772 do not accept a resin yellow card as substitute for end-product testing. The addition ratio for this grade in the insulating shell is 100 wt%; regrind is limited to 5 wt% or eliminated entirely because glass-fiber attrition in thin-wall regrind reduces tensile strength and increases black speck defects on visible charge inlet faces. Drying is performed at 120 °C for 4–5 h to moisture below 0.02%; melt temperature is set between 255 °C and 265 °C, with mold temperature 90–100 °C because thin-walled parts depend on high mold temperature to complete crystallization before ejection. Injection velocity is set to produce a fill time of 0.5–1.5 s for flow lengths above 100 mm; holding pressure is switched by screw position, not timer, with cushion 4–6 mm and decompression 3 mm. The processing window is narrow: melt temperatures above 270 °C lead to visible silver streaking from flame-retardant decomposition, while temperatures below 250 °C risk short shots in thin ribs and bosses. After unscheduled line stoppages, barrel temperature is reduced to 230 °C to limit degradation in the screw channel before restart. Published data for V-0 performance at wall thickness below 0.8 mm for this specific product family is limited, so each geometry must be tested by IEC 60695-11-10 or UL 94 on molded plaques of the same thickness. The final articles are CCS2 charge inlet housings, on-board charger control carriers, and DC fast-charge connector shells.
| Application | Standard | Test method / clause | End-product criterion |
|---|---|---|---|
| Low-voltage switchgear | IEC 60664-1, IEC 60947-1 | IEC 60112 comparative tracking index; UL 94 vertical burn | Insulation coordination for rated impulse voltage; no tracking at creepage distance |
| Automotive underhood | SAE/USCAR-2 Rev 7, LV214-1 | Vibration and thermal cycling sequences; terminal retention force | Retention force above OEM minimum after environmental exposure |
| Household appliance | IEC 60335-1, IEC 60695-2-11 | Clause 30.2.3.1 glow-wire end-product test | No ignition or self-extinguish within specified time on final part |
| EV charging | IEC 61851-1, IEC 62196-2, UL 2251, SAE J1772 | IEC 60695-11-10 thin-wall flame test; end-product dielectric | Flame class on actual geometry; dielectric withstand after thermal cycling |
| Industrial contactors | UL 508, IEC 60947-4-1 | Impact after molding; arc-chamber dimensional stability | Mechanical endurance and dielectric integrity after operations |
| Power tools | IEC 62841-1, UL 62841-1 | Insert retention; post-anneal UL 94 V-0 check | Double-insulation spacing and commutator alignment maintained |
Large-frame industrial contactors and motor starters are often evaluated under UL 508 and IEC 60947-4-1; the resin's contribution is through dimensionally stable arc chamber partitions after tens of thousands of electrical operations and thermal cycles. In this conversion step the compound is metered at 100 wt% of the polymer; if regrind is reused from thick-walled sprues, the proportion is kept at 20 wt% maximum and the resulting impact strength is checked by ISO 179-1/1eA or ASTM D256 because glass fiber length reduction lowers energy absorption in deep rib bases. The pre-drying step is identical to other glass-filled PBT conversion: 120 °C for 4 h in a dry-air dryer to 0.02% moisture. Injection molding uses a screw with L/D 20:1 and compression ratio 2.0:1, barrel temperatures from 245 °C to 260 °C, and mold temperature 85–95 °C; sequential valve gating or hot-runner valve gates are used for large contactor bases to avoid visible knit lines in areas adjacent to the moving armature. Hold pressure is maintained until the gate freezes, with final cushion 3–5 mm. The terminal parts are contactor arc chute supports, relay mounting bases, and motor starter coil formers.
Insert molding of brass commutator rings and brush holder plates in hand-held power tools is controlled by IEC 62841-1 and UL 62841-1, with critical failure modes being brush-tube misalignment after high-speed rotation and stress cracking around the insert. The compound is molded at 100 wt% as supplied; no unfilled PBT is added to improve flow because this would lower the glass content below the formulation on the yellow card and shift mold shrinkage outside the compensated tool dimensions. Brass inserts are preheated to 100 °C to 120 °C and inserted just before shot start; the mold temperature is held at 60–90 °C to keep cycle time short while maintaining adequate surface flattening around the insert. Barrel set points are 245 °C rear to 260 °C nozzle; the screw uses L/D 20:1 and a compression ratio of 2.0:1 to limit shear heating. Post-mold dimensional stabilization, if required for high-precision commutator brackets, is carried out at 120 °C for 1–2 h only after verifying that flame-retardant migration to the surface does not increase smoke or reduce UL 94 V-0 on the post-annealed part. The resulting components are brush card holders, commutator brackets, and armature end caps for class II double-insulated power tools.
Competitive SABIC VALOX™ PBT-FR 420SE0-BK1066 prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
SABIC VALOX™ PBT-FR 420SE0-BK1066 is a 30% short-glass-fiber-reinforced polybutylene terephthalate injection molding compound supplied in black. The BK1066 suffix identifies a carbon-black-containing color package rather than a separate polymer chemistry. The grade carries a UL 94 V-0 flame-retardant classification at 1.5 mm nominal wall thickness and is specified for connector housings, relay bases, switch bodies, bobbins, motor end caps, and power-distribution components in which dimensional stability and self-extinguishing behavior are load-bearing requirements. Under ISO 527-2/5, tensile stress at break is 120 MPa and tensile strain at break is 3.0%. Under ISO 178, flexural modulus is 9000 MPa and flexural strength is 175 MPa. Density under ISO 1183-1:2019 is 1.62 g/cm³. Heat deflection temperature under ISO 75-2/Af at 1.8 MPa is 200°C. Mold shrinkage under ISO 294-4 is 0.3–0.5% in the flow direction. Published data specific to the BK1066 color balance are limited relative to natural 420SE0; colorant-associated shifts in notched impact and surface electrical properties should be confirmed lot by lot.
| Property | Test standard | Typical value |
|---|---|---|
| Density | ISO 1183-1:2019 | 1.62 g/cm³ |
| Tensile stress at break | ISO 527-2/5 | 120 MPa |
| Tensile strain at break | ISO 527-2/5 | 3.0% |
| Flexural modulus | ISO 178 | 9000 MPa |
| Flexural strength | ISO 178 | 175 MPa |
| Notched Izod impact at 23°C | ISO 180/A | 8.0 kJ/m² |
| Heat deflection temperature at 1.8 MPa | ISO 75-2/Af | 200°C |
| Mold shrinkage, flow direction | ISO 294-4 | 0.3–0.5% |
| Flammability at 1.5 mm | UL 94 | V-0 |
| Comparative tracking index | IEC 60112 | 250 V |
The transition from unfilled PBT-FR to 30% glass fiber creates a matrix-to-fiber load-transfer system whose tensile and flexural response is governed by fiber orientation. A representative unfilled flame-retardant PBT exhibits tensile stress at yield near 55–60 MPa and flexural modulus near 2500–2800 MPa; 420SE0 raises tensile stress at break to 120 MPa and flexural modulus to 9000 MPa, a stiffness increase of approximately 3.2×. This gain is accompanied by reduced ductility: tensile strain at break is 3.0%, while unfilled PBT commonly elongates by more than 50%. For snap-fit or post-assembly deformation, the low elongation limit of 420SE0 becomes the design boundary. Mold shrinkage also changes fundamentally: unfilled PBT exhibits shrinkage above 1.5%, whereas 420SE0 shows 0.3–0.5% in the flow direction under ISO 294-4. Cross-flow shrinkage is typically higher because transverse fiber orientation constrains volumetric contraction less effectively than flow-direction alignment. Weld-line tensile strength in glass-filled PBT is normally below the matrix-only value; at knit lines, fiber ends do not bridge the flow front and the local failure path follows the unfilled matrix. Multi-gate tools therefore require gate-positioning analysis that places weld lines outside primary load paths.
Fiber orientation in the skin layer follows melt velocity vectors; in the core of thicker sections, fibers may rotate transverse to flow. This shell-core structure creates a modulus gradient across the wall that cannot be represented by a single isotropic finite-element property set derived from datasheet values. In edge-gated plaques, flow-direction flexural modulus can exceed cross-flow modulus by 15–30%, but published data for this specific BK1066 compound in complex multi-cavity housings are limited. Orientation-dependent modulus should be measured from actual moldings machined into bars tested at 0° and 90° to the primary flow direction under ISO 527-2 before load-bearing simulations are accepted.
Maintaining fiber length during screw plastication requires a general-purpose or low-shear injection screw with an L/D ratio of at least 20:1 and a compression ratio near 2.5:1. Barrel temperatures are profiled from hopper to nozzle so that melt temperature at the nozzle is held between 250°C and 270°C; sustained temperatures above 270°C accelerate ester hydrolysis and flame-retardant decomposition, producing black speck formation in the BK1066 color package. Mold temperature is set between 60°C and 100°C to balance crystallization rate and surface appearance. A desiccant-bed dryer with air dew point at or below −30°C is used at 120°C for 3–4 h; residual moisture must be below 0.02 wt% before plastication. If hopper residence under ambient relative humidity above 60% exceeds 1 h, surface moisture re-uptake can exceed the processing limit and cause hydrolysis, loss of tensile strength, and visible splay. Back pressure is limited to 0.3–0.7 MPa to avoid over-working the glass-fiber network; screw rotation speed is typically capped at 100 rpm on a 36:1 L/D general-purpose screw. Cushion decompression after plastication is held to the minimum that prevents nozzle drool because excessive decompression pulls air into the melt cushion and contributes to gate splay.
| Processing parameter | Condition or requirement | Reference value or equipment type |
|---|---|---|
| Drying equipment | Desiccant-bed dryer | Air dew point ≤ −30°C |
| Drying temperature | Inlet air temperature | 120°C |
| Drying time | Closed-loop desiccant drying | 3–4 h |
| Residual moisture | Maximum before plastication | 0.02 wt% |
| Melt temperature at nozzle | Barrel profile range | 250–270°C |
| Mold temperature | Fixed and moving halves | 60–100°C |
| Back pressure | Screw recovery | 0.3–0.7 MPa |
| Screw speed | General-purpose screw | 50–100 rpm |
| Screw geometry | L/D ratio and compression ratio | ≥ 20:1, 2.5:1 |
| Maximum melt residence time above 270°C | Flame-retardant stability limit | 5 min |
Gate freeze-off in glass-filled PBT is sensitive to mold temperature; at the lower end of the 60–100°C mold-temperature range, small subgates may freeze before full packing pressure is transferred to the part. Cavity-pressure sensors placed just after the gate can establish the gate-seal time; hold pressure is effective only until gate solidification. For thick bosses and ribs, pack-pressure decay after gate seal no longer controls shrinkage, and part mass becomes the more reliable process control parameter than hold-pressure timer settings.
Hot-runner systems for 420SE0 should use externally heated manifolds with open-pipe melt channels and no dead spots. Glass fibers are abrasive; screw flight lands, check rings, and barrel liners should be through-hardened or bimetallic. The documented processing window assumes a clean feedstock stream; contamination with amorphous resins such as polycarbonate or with hygroscopic polyamide can delaminate the PBT matrix and should be avoided. Published data for hot-runner pressure drop in this specific BK1066 grade are limited; rheological data should be collected on the intended manifold geometry.
Under ISO 75-2/Af at 1.8 MPa, the heat deflection temperature is 200°C; this result permits short-term soldering and reflow exposure if the part is not under mechanical load at peak temperature. Continuous service under load at 200°C is not implied by HDT/A. Comparative tracking index under IEC 60112 is 250 V, which supports low-voltage switch and relay applications when creepage distances are selected according to IEC 60664-1. Volume resistivity is generally high for PBT, but the BK1066 carbon-black package can alter surface resistivity; nonconductive and conductive black formulations are not equivalent. The UL 94 V-0 classification is thickness-dependent; parts with walls below 1.5 mm require evaluation against the specific thinner-wall listing or independent testing because thickness and gassing can shift the flame outcome. In continuous service, the ester linkages of PBT are hydrolytically sensitive; exposure to hot aqueous media above 60°C can degrade molecular weight and mechanical integrity even if the part passes dry-heat aging.
Tooling and process conditions determine whether the published mold shrinkage can be delivered as a process capability above Cpk 1.33. The glass-fiber orientation distribution is not isotropic; cavity filling must be balanced by runner and gate sizing, and volumetric fill imbalance between cavities should be held below 5%. Mold temperature uniformity across the fixed and moving halves is maintained within ±5°C, because local cooling variation shifts semicrystalline PBT shrinkage by several tenths of a percent. Holding pressure is staged to compensate for gate freeze-off; hold time should be validated by weight-stability studies rather than by nominal timer settings. Parts ejected above 100°C can exhibit post-mold shrinkage after measurement, so dimensional validation should occur at a standardized post-molding time, such as 48 h after molding under ISO 291 atmosphere. Cavity-to-cavity and shot-to-shot variation must be quantified in first-article layout because published data for the BK1066 color package in multi-cavity tooling are limited.
Storage in sealed containers at ambient relative humidity below 60% is standard for lot-to-lot consistency; if bags are opened in humid environments, drying must be repeated before molding. The flame-retardant system in a glass-filled PBT-FR grade may contain a halogenated synergist or antimony compound; the supplier’s REACH SVHC declaration and the specific application’s RoHS obligations should be verified before shipment because additive changes can alter the declaration. This information is not a legal compliance certification for an end-use assembly. The material is not intended for food-contact use unless validated under FDA 21 CFR or equivalent regional migration testing.