| HS Code | 331074 |
| Materialtype | PBT, 30% glass fiber reinforced, flame retardant, UV stabilized |
| Color | Black |
| Density | 1.53 g/cm³ |
| Tensilemodulus | 11000 MPa |
| Tensilestressatbreak | 120 MPa |
| Tensilestrainatbreak | 2.0% |
| Flexuralmodulus | 10500 MPa |
| Flexuralstrength | 180 MPa |
| Notchedizodimpactat23c | 8 kJ/m² |
| Hdtat1 82mpa | 200 °C |
| Hdtat0 45mpa | 210 °C |
| Vicatsofteningtemperature | 215 °C |
| Ul94flammabilityrating | V-0 at 0.75 mm |
| Waterabsorption | 0.1% |
| Moldingshrinkageflow | 0.2-0.5% |
| Moldingshrinkagecrossflow | 0.6-0.9% |
| Volumeresistivity | >1E15 ohm·cm |
| Dielectricstrength | 20 kV/mm |
As an accredited SABIC VALOX™ PBT-FR 357U BK1066 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | SABIC VALOX™ PBT-FR 357U BK1066 is packaged in 25 kg moisture-barrier bags, palletized for safe industrial storage and transport. |
| Container Loading (20′ FCL) | 20′ FCL container loading: SABIC VALOX™ PBT-FR 357U BK1066 in palletized bags, shrink-wrapped and secured for safe ocean transport. |
| Shipping | Ship SABIC VALOX™ PBT-FR 357U BK1066 in original sealed, moisture-barrier packaging—typically 25 kg bags or 1,000 kg octabins—under dry, ambient conditions. Protect from moisture, heat, UV, and punctures. Normally non-hazardous for transport; always follow the SDS and applicable DOT/IMDG/IATA regulations. |
| Storage | Store SABIC VALOX™ PBT-FR 357U BK1066 in a cool, dry, well-ventilated warehouse away from direct sunlight, heat sources, open flames, and moisture. Keep material in original, sealed, clearly labeled packaging or containers. Prevent exposure to incompatible chemicals and ignition sources. Use first-in/first-out stock rotation and follow the manufacturer’s SDS and local storage regulations. |
| Shelf Life | Shelf life is generally 24 months when kept in original sealed packaging, cool, dry, and protected from moisture and sunlight. |
In multi-cavity board-to-wire connector tools, the unfilled flame-retardant PBT is processed at a melt temperature of 240°C to 260°C and a mould temperature of 60°C to 80°C. Pre-drying in a desiccant dryer at 120°C for 3 h to 4 h with a dew point below -40°C is mandatory because residual moisture above 0.02% hydrolyzes the PBT backbone during plastication, lowering molecular weight and producing inconsistent fill pressure at the transfer point. On a 24-cavity valve-gated hot-runner tool, batch-to-batch variation in the flame-retardant package appears as shifts in melt viscosity that require adjustment of the hold-pressure profile; regrind content above 20% is not recommended because viscosity drift and colour change become more difficult to control. The mould shrinkage band under ISO 294-4 is 0.8% to 1.0% in the flow direction, and gate freeze must be confirmed by sequential screw-position pressure-drop measurements before the tool is qualified for dimensional capability. Connector housings with wall thickness below the UL Yellow Card minimum thickness lose the UL 94 V-0 classification; the design should therefore maintain the rated minimum wall in all areas between adjacent live terminals, including the thin diaphragm at the bottom of the terminal cavity. Short-shots are frequently misattributed to low melt temperature when the actual cause is insufficient drying before the screw plastication zone reaches thermal equilibrium, because acidic hydrolysis products reduce melt elasticity and cause filling instability in thin ribs.
Because terminal blocks operate in enclosures rated pollution degree 2 with adjacent live parts, the comparative tracking index of the moulded insulator determines the creepage distance selected under IEC 60664-1:2020. The test method in IEC 60112:2020 applies an electrolyte of 0.1% ammonium chloride in deionized water with a drop interval of 30 s and a total of 50 drops between two platinum electrodes spaced 4 mm apart. Unreinforced flame-retardant PBT grades can produce conductive carbonized paths during tracking tests; because the grade is unfilled, the absence of glass fibres prevents mechanical reinforcement of the carbonised path, which is one of the determinants of the CTI band. Designers must obtain the CTI value from the current UL Yellow Card for BK1066, and their creepage calculations should not substitute a generic PLC 0 or PLC 1 value. Under IEC 60664-1, a lower CTI class moves the required creepage distance upward for a given working voltage and pollution degree, particularly in terminal blocks installed in industrial control panels. When the terminal block contains adjacent live parts with a working voltage above 250 V, creepage distances derived from a lower CTI class may be 1.5 to 2.0 times those for a higher CTI class; the exact value must be selected from the relevant standard table rather than a single generic clearance formula. In practice, terminal block housings are moulded with barriers between poles that serve as creepage extensions. The barrier height, draft angle, and surface roughness after mould wear all influence the effective creepage path, because a rough surface retains conductive dust and reduces tracking resistance in service. Moulders should therefore control mould release agent usage; external mould release sprays can lower surface resistivity and alter CTI performance, especially on black-coloured parts where contamination is less visible.
A narrow processing window between adequate thin-wall filling and flame-retardant decomposition dominates the moulding of relay sockets with wall sections as low as 0.5 mm around terminal receiving apertures. A conventional three-zone reciprocating screw with 20:1 to 24:1 L/D and a low compression ratio of 2.0:1 to 2.5:1 is preferred. Barrel temperatures are profiled from 240°C at the rear zone to 260°C in the metering zone, with the nozzle maintained at 255°C. Screw back pressure should remain between 0.3 MPa and 0.7 MPa; higher back pressure raises melt residence time and shear heating, which accelerates plate-out from the brominated flame-retardant package. On production-scale tools cycling at 25 s to 35 s, plate-out commonly appears first on the mould core near venting grooves after 6 h to 8 h of continuous operation. The deposit increases ejection force and creates surface drag marks on the relay socket sidewall. Mould temperature should be held at 60°C to 80°C, with cavity-to-cavity uniformity within ±5°C because uneven mould surface temperature causes differential shrinkage between the thin terminal apertures and the thicker base plate. Thin-wall relay sockets with nominal wall thickness 0.5 mm require elevated injection velocities and packing pressures in the range 50 MPa to 80 MPa; however, excessive packing pressure with slow screw recovery can increase gate blush and part warpage. The unfilled grade’s low melt elasticity also means that venting depth should not exceed 0.02 mm to avoid flash. Table 1 summarises the processing window.
| Processing parameter | Setting | Equipment or test basis |
|---|---|---|
| Drying temperature / time | 120°C / 3 h–4 h | Desiccant dryer, dew point ≤ -40°C |
| Residual moisture target | <0.02% | Karl Fischer titration |
| Melt temperature | 240°C–270°C | Nozzle thermocouple |
| Mould temperature | 40°C–80°C | Water or oil mould heater |
| Back pressure | 0.3 MPa–0.7 MPa | Hydraulic or electric injection unit |
| Injection speed | Medium to high | Fill time 0.5 s–1.5 s |
| Holding pressure | 50 MPa–80 MPa | Injection moulding machine |
If an appliance control housing carries current or is fitted to unattended equipment, the glow-wire end-product assessment in IEC 60695-2-11:2021—not the raw-material UL 94 plaque classification—determines compliance. A control housing that supports current-carrying parts may be tested at a glow-wire tip temperature of 850°C according to IEC 60335-1:2020 subclause 30.2.3, depending on the current and the presence of an unattended operating mode. The test applies a heated wire to the finished moulded surface for 30 s; the material must not ignite, or if ignition occurs the flame must extinguish within 30 s after the wire is withdrawn and the tissue paper layer below must not ignite. Unfilled flame-retardant PBT can meet this requirement at nominal wall thickness of 1.5 mm to 3.0 mm when the part is free of weld lines in the contact area and the mould surface has not been contaminated with release agents. Because BK1066 is a black formulation, carbonaceous deposits from long moulding runs can mask early signs of flame-retardant degradation; end-product glow-wire tests should be repeated after the tool has run 5,000 to 10,000 shots if visual inspection is the only in-process control. Ball-pressure testing under IEC 60695-10-2 uses a 5 mm diameter steel sphere at a load of 20 N for 1 h; the indentation diameter must not exceed 2 mm. For parts supporting live connections in appliances, the ball-pressure temperature is typically 125°C. The unfilled grade’s heat deflection temperature of approximately 60°C at 1.8 MPa by ISO 75-2 means that continuous load-bearing contact with metal terminals above 75°C can cause localised creep and loss of contact force; the application should therefore be thermally mapped before replacing glass-reinforced PBT in high-current appliance circuits.
After prolonged solar exposure, outdoor terminal strip insulators and distribution box covers require re-qualification of surface tracking resistance because the ultraviolet-stabilised PBT may undergo surface oxidation that changes wetting behaviour. The U designation in VALOX PBT-FR 357U BK1066 indicates an ultraviolet-stabilised formulation, but the stabiliser package protects surface gloss, base tensile properties, and colour shift rather than serving as an unconditional long-term weathering warranty. Accelerated xenon arc weathering under ISO 4892-2:2013 cycle 1A uses a black standard temperature of 65°C and an irradiance of 0.35 W/m² at 340 nm. Published data for this specific grade after outdoor terminal strip service is limited; end-product validation should include surface resistivity and comparative tracking index retention after 1,000 h of xenon arc exposure because surface oxidation can alter wetting behaviour and accelerate tracking. Moulders should not infer UV stability from an unexposed UL 94 Yellow Card rating; flame-retardant additives can migrate or undergo surface modification under UV, and the part’s dielectric performance must be re-tested on aged samples. Where terminal strips are installed inside an enclosure with a transparent cover, the UV load is filtered, but heat build-up may still exceed the grade’s electrical relative thermal index. The unfilled material should not be specified for load-bearing outdoor insulators at continuous temperatures above 75°C unless creep testing on the actual part geometry demonstrates acceptable dimensional stability.
Measured dielectric performance on actual switchgear arc barriers, rather than standard plaque values, should drive the design because wall thickness and flow-line location influence breakdown strength. Arc barriers in low-voltage switchgear are moulded at wall thicknesses of 1.5 mm to 3.0 mm to separate live busbars and attenuate arc flash propagation. The unfilled flame-retardant PBT is selected where the barrier must carry no continuous structural load but must satisfy dielectric strength and flame resistance simultaneously. UL 94 5VA classification, when applicable at 3.0 mm according to the Yellow Card, is relevant for enclosures required to resist burn-through after flame impingement; the black BK1066 colour is part of the rated configuration and should not be assumed equivalent to natural or custom-coloured compounds. The insulating barrier design should avoid sharp internal corners at mounting bosses because the unfilled grade’s notched impact strength is lower than glass-reinforced PBT; radiused transitions of 1.0 mm to 1.5 mm and generous flow leaders reduce crack initiation after screw torque installation. Processors have reported ejection cracking in flat barriers when the mould opens before the part reaches ejection temperature; a mould temperature of 60°C to 80°C and holding pressure sufficient to prevent sink marks at gate locations are necessary. The material’s dielectric strength under IEC 60243-1 should be verified on the actual part thickness, because thin sections near flow lines can create local weakness. This application is not suitable for continuous operating temperatures above 75°C unless the barrier is mechanically supported, because unfilled PBT under load will creep near its heat deflection temperature.
Competitive SABIC VALOX™ PBT-FR 357U BK1066 prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
SABIC VALOX™ PBT-FR 357U BK1066 is a flame-retardant, unreinforced polybutylene terephthalate resin supplied as black pellets with a UV-stabilised colour package. The product is specified for injection-moulded electrical and electronic components that must meet UL 94 V-0 at 0.71 mm nominal wall thickness, including terminal housings, relay bases, switch frames, connector insulators, and appliance control enclosures. Because the resin is unfilled, melt viscosity is lower than that of glass-filled PBT grades, and mould shrinkage measured according to ISO 294-4 is generally more isotropic in multi-gate tools. Tensile modulus, tensile-creep resistance, and deflection temperature under load are lower than those of 30% glass-reinforced VALOX 420SEO. The black BK1066 package provides ultraviolet stabilisation for indoor exposure to fluorescent light and filtered sunlight. Design calculations should be based on the current SABIC technical datasheet and lot-specific certificate of analysis rather than on class-average PBT values.
| Property | Test method | Typical value |
|---|---|---|
| Density | ASTM D792-20 | 1.41 g/cm³ |
| Tensile stress at yield, Type I | ASTM D638-14 | 50 MPa |
| Tensile elongation at break | ASTM D638-14 | 4.0 % |
| Flexural strength | ASTM D790-17 | 82 MPa |
| Flexural modulus | ASTM D790-17 | 2,300 MPa |
| Notched Izod impact, 23 °C | ASTM D256-10 Method A | 24 J/m |
| Deflection temperature under load, 0.45 MPa | ASTM D648-18 | 160 °C |
| Flammability, 0.71 mm | UL 94 | V-0 |
The values are representative of the product class and may shift with colour lot, moisture state, or regrind content. For mould-flow simulation, a grade-specific shear-viscosity curve should be entered; substitution of a generic unfilled PBT viscosity model can underestimate thin-wall filling pressure. Published data for this specific configuration is limited, and 0.35 mm wall certification should be confirmed against the UL yellow card.
PBT hydrolyses at melt temperature when residual moisture exceeds 0.02 wt%. The granules should be dried in a desiccant dryer with a dew point no higher than −30 °C at 120 °C for 3 h to 4 h. At ambient relative humidity above 60%, the hopper should be closed and purged with dry air or nitrogen, with exposed granulate residence limited to 30 min. Residual moisture should be verified by Karl Fischer titration according to ISO 15512. Wet material produces silver streaking, loss of notched impact, and a measurable drop in tensile strength from hydrolytic chain scission; re-drying can remove free moisture but cannot restore molecular weight already lost.
The melt temperature measured at the nozzle should be kept between 245 °C and 260 °C. Prolonged residence beyond 5 min at 260 °C causes decomposition of the brominated flame-retardant package and deposition of acidic degradation products on the tooling. A barrel profile of 230 °C feed, 240 °C compression, 250 °C metering, and 240 °C nozzle is typical for a reciprocating-screw injection machine with L/D of 18:1 to 22:1 and compression ratio between 2.5:1 and 3.0:1. Shot weight should be between 30% and 70% of barrel capacity. Mould temperature should be maintained from 40 °C to 80 °C; for wall thickness below 1.0 mm, the lower portion of the range may produce premature skin solidification and should be avoided.
The grade is susceptible to jetting when a small gate exits into an open cavity. Edge gates should have a depth of 60% to 80% of wall thickness and a width of at least 1.5 mm. Submarine or pin-point gates below 1.0 mm diameter are not recommended unless the melt is discharged against a wall or obstruction. Hot-runner tools should use open-pipe flow channels without dead-end pockets; manifold temperature should be held near 245 °C, and heaters should be verified by thermocouple placement to avoid local excursions above 260 °C.
Regrind use should be limited to 20 wt% and mixed only with dry virgin material from the same lot. Regrind containing degraded sprue, purgings, or material from a machine that previously processed glass-filled PBT should not be introduced into the hopper. The melt-viscosity shift of regrind is measurable by melt volume-flow rate under ISO 1133-1 at 250 °C and 2.16 kg, but the target value is grade-specific and should be established in initial lot qualification.
In replacing a non-flame-retardant PBT with VALOX PBT-FR 357U BK1066, the main process changes are the need for tighter moisture control and the lower upper melt-temperature tolerance caused by the flame-retardant package. The non-flame-retardant VALOX 357U grade does not carry the same UL 94 V-0 classification at 0.71 mm. The flame-retardant additive system generally reduces tensile elongation at break and notched impact relative to a non-flame-retardant unfilled PBT of equivalent molecular weight; snap-fit features should be evaluated by ASTM D638-14 and ASTM D256-10 rather than by flexural testing alone. The use of amine-based mould release agents, amine-containing colourants, or amine-containing antistatic additives is to be avoided because amines accelerate flame-retardant decomposition and tooling plate-out.
The unfilled structure of VALOX PBT-FR 357U BK1066 gives a lower flexural modulus, lower tensile strength, and lower deflection temperature under load than the 30% glass-fibre-reinforced VALOX 420SEO grade. When assessed by ASTM D790-17, the glass-filled grade may exhibit flexural modulus roughly 2.5 times to 3 times higher than the unfilled grade; the exact ratio depends on specimen conditioning and fibre orientation. The unfilled material has better flow length under identical screw pressure, reduced fibre-rich surface layers, and lower anisotropic shrinkage as measured by ISO 294-4. Weld-line regions in glass-reinforced PBT often show a greater loss in tensile strength because glass fibres do not cross the knit-line efficiently; the unfilled grade may retain a higher fraction of its tensile strength across a weld line, although the absolute weld-line strength remains below the bulk value.
Comparative tracking index measurements made according to IEC 60112 can differentiate the two materials in electrical applications. Glass fibre at the moulded surface can create high local surface resistivity and lower tracking performance; unfilled flame-retardant PBT may therefore be selected where IEC 60112 requirements above 250 V must be demonstrated. Electrical creepage and clearance distances should still be calculated from the end-use pollution degree and CTI class under IEC 60664-1. For load-bearing mechanical parts, glass-reinforced VALOX 420SEO is preferred because its higher modulus and higher heat-deflection temperature maintain clamp force and dimensional stability under load.
| Parameter | Standard / method | Position |
|---|---|---|
| Flammability | UL 94 | V-0 at 0.71 mm |
| Comparative tracking index | IEC 60112 | Minimum 250 V when lot-certified; dry laboratory values may not represent field weathering |
| Residual moisture | ISO 15512 | 0.02 wt% maximum before processing |
| Restriction of hazardous substances | EU 2011/65/EU recast | Supplier declaration required; analytical verification by XRF may not detect all brominated species |
| Food-contact | FDA 21 CFR 177.1660 | Not supplied as a food-contact grade unless a dedicated compliance letter is issued |
When the product is used for thin-wall housings with nominal wall thickness below 0.8 mm, the limiting variables are not the melt flow alone but the solidification layer growth rate and the pressure required to pack the far edge of the cavity. Mould temperatures below 50 °C can create a thick frozen skin that extends into the flow channel and causes short shots in unfilled flame-retardant PBT. A mould temperature of 60 °C to 80 °C should be maintained, and sequential valve gating should be used when flow length-to-thickness ratio exceeds 120:1. Packing pressure should be applied for a duration just sufficient to eliminate sink marks; overpacking at the gate increases residual stress and can cause warpage after annealing.
Thin-wall parts may require high injection speeds to prevent hesitation at ribs and boss features. The use of a profiled injection velocity is recommended: slow initial advance across the sprue, high velocity for the primary flow path, and reduced velocity near the end of fill to avoid gas entrapment. Venting depth should be limited to 0.02 mm to 0.03 mm for PBT; deeper vents encourage flash. Cavity pressure transducers are the most reliable method to control switchover from velocity control to pressure control, with switchover at 95% of fill volume as a starting point. Process validation should include short-shot progression studies and cross-section analysis of weld lines rather than reliance on injection pressure alone.
Because the flame-retardant package is thermally sensitive, hot-runner start-up should limit total melt residence time in the manifold to 5 min at 250 °C. After a production interruption longer than 10 min, the hot-runner manifold should be held at 230 °C and purged with a non-flame-retardant PBT until the system is free of degraded melt. The purge material should not be mixed back into regrind. Use of closed-loop mould temperature control with water or oil units is preferred to detect flow-channel blockage early. If a thermal gate is used, the tip temperature should be controlled independently to avoid exceeding 260 °C during the gate-opening pulse.