| HS Code | 377513 |
| Density | 1.31 g/cm³ (typical) |
| Melt Volume Rate 250 C 2 16 Kg | 10 cm³/10 min (typical) |
| Tensile Modulus | 2300 MPa (typical) |
| Tensile Stress At Yield | 50 MPa (typical) |
| Tensile Strain At Yield | 5% (typical) |
| Flexural Modulus | 2200 MPa (typical) |
| Notched Izod Impact Strength 23 C | 20 kJ/m² (typical) |
| Notched Izod Impact Strength 30 C | 10 kJ/m² (typical) |
| Hdt At 0 45 Mpa | 150°C (typical) |
| Hdt At 1 8 Mpa | 85°C (typical) |
| Vicat Softening Temperature | 160°C (typical) |
| Ul94 Flame Rating | V-0 at 1.5 mm |
| Coefficient Of Linear Thermal Expansion Flow | 7×10⁻⁵ cm/cm/°C (typical) |
| Molding Shrinkage Flow | 0.5–0.8% (typical) |
As an accredited SABIC VALOX™ Impact-Modified PBT 357X factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | SABIC VALOX™ Impact-Modified PBT 357X is typically supplied in 25 kg moisture-resistant bags, palletized for industrial storage and handling. |
| Container Loading (20′ FCL) | Standard 20-foot FCL dry container loaded with palletized SABIC VALOX™ Impact-Modified PBT 357X resin, securely stowed for ocean freight. |
| Shipping | SABIC VALOX™ Impact-Modified PBT 357X ships as resin pellets in sealed 25-kg bags or octabins, palletized and shrink-wrapped. Transport in dry, ventilated conditions, protected from moisture, heat, direct sunlight, and contamination. Use original packaging, avoid punctures, and follow the SDS and local transport regulations. |
| Storage | Store SABIC VALOX™ Impact-Modified PBT 357X in a cool, dry, well-ventilated area away from direct sunlight, heat, sparks, and open flames. Keep containers tightly closed and protect from moisture, contamination, and physical damage. Maintain good housekeeping and avoid dust generation. Store away from incompatible substances, keep packaging sealed until use, and follow the manufacturer’s SDS and local regulations. |
| Shelf Life | SABIC VALOX™ Impact-Modified PBT 357X has a shelf life of 24 months when stored dry, cool, and in original sealed packaging. |
Within the engine compartment, under-hood electrical connector shells, secondary locking features, and wire dress clips are molded from SABIC VALOX™ Impact-Modified PBT 357X where the specification requires dimensional stability after heat aging and ductile failure during snap-fit insertion. The resin is pre-dried in a desiccant dryer with a supply air dew point of -40 °C and a bed temperature of 120 °C for 4 h, bringing moisture content below 0.02 % by weight before melt processing; moisture analysis is conducted by ISO 15512. Processing on a 20:1 L/D reciprocating screw injection molding machine with a shut-off nozzle uses rear-zone 235 °C, mid-zone 245 °C, front-zone 250 °C, and nozzle 255 °C, while the mold surface temperature is held at 80 °C to promote crystallization in snap-fit living hinges. The gate is placed away from pin-adjacent weld lines because knit-line retention strength in impact-modified PBT is lower than the surrounding bulk even when the notched Izod value measured by ISO 180/A at 23 °C is acceptable. Dimensional acceptance for connector pitch is based on ISO 294-4 shrinkage plaque data, and thermal aging resistance is compared after 1000 h exposure at 120 °C using tensile retention per ISO 527-2. For USCAR-2 connector validation, the part is subjected to thermal shock between -40 °C and 85 °C with vibration profiles specific to the OEM, and cracking at the secondary lock beam is the rejection criterion. Fluid immersion testing commonly includes engine oil, transmission fluid, and road salt mist, with visual inspection for stress cracking after 24 h annealed aging at 80 °C; PBT impact-modified grades are not recommended for sustained exposure to hot engine coolant above 90 °C because hydrolysis-induced molecular weight loss reduces impact strength. Published data for this specific grade in aggressive hot coolant immersion is limited, so validation at the final wall thickness and injection stress level is required before qualification.
| Assessment | Standard or method | Test condition |
|---|---|---|
| Moisture after drying | ISO 15512 | 0.02 % maximum |
| Notched Izod impact | ISO 180/A | 23 °C |
| Tensile strength retention after aging | ISO 527-2 | 120 °C, 1000 h |
| Comparative tracking index | IEC 60112 | Reported per production mold |
The transition from die-cast metal to impact-modified PBT in double-insulated power tool housings places the vibration weld joint at the perimeter of a structural shell that must survive drop testing onto concrete from 2 m at -10 °C after conditioning per IEC 60745-1 and IEC 62841-1. The 357X grade is processed with a melt temperature of 245 °C to 255 °C and a mold temperature of 60 °C to 80 °C, with hold pressure adjusted to minimize sink marks at the screw bosses and avoid overpacking the weld joint shear zone. The impact modifier phase reduces stiffness relative to glass-filled PBT, so the housing rib pattern must be designed with a mass moment of inertia sufficient to keep deflection under a 500 N clamp load below the clearance for the armature bearing. Vibration welding amplitude of 0.8 mm to 1.2 mm at 200 Hz is used on a linear vibration welder, and the weld strength is checked by sectioning and pull testing across the weld bead. Because the material is semi-crystalline, the weld flash is relatively brittle compared with an amorphous polycarbonate weld flash, and the joint design should use a shear joint rather than a butt joint to displace flash outward without reducing wall thickness. Electric motor end bells and gear housings are terminal parts that require creep resistance under continuous operating temperatures up to 110 °C when the motor is stalled; published creep data for this specific impact-modified grade at those temperatures is limited, so bolted joint clamping force retention must be tested on prototype cavity steel rather than extrapolated from short-term tensile creep. UL 94 classification for the housing should be confirmed on the production wall thickness because the impact-modifier package can alter the burning behavior relative to unmodified PBT; any use of an external flame retardant masterbatch requires reassessment of weldability.
Inside industrial control cabinets, terminal blocks and relay sockets are molded from VALOX 357X because the material provides dimensional control across multi-cavity tools and a low post-molding shrinkage anisotropy when melt temperature is kept at 250 °C and mold temperature at 80 °C. The primary electrical safety assessment for these parts is the comparative tracking index under IEC 60112 solution A, and the insulation coordination distances are verified according to IEC 60664-1 for overvoltage category II or III depending on the cabinet location. Glow-wire testing per IEC 60695-2-11 is conducted at 750 °C or 850 °C on the final wall thickness, and the result is reported as either ignition temperature via IEC 60695-2-13 or flammability index via IEC 60695-2-12. The terminal block screws, metal inserts, and snap-on DIN rail latching hooks impose local stress concentrations, so the gate is placed on the latch rib to orient flow lines away from the insertion force edge; a hot-tip valve gate is preferred over a cold runner because the material’s crystalline solidification can produce visible flow hesitation when the melt enters a cold runner below the no-flow temperature. Long-term thermal aging at 85 °C for 5000 h in an air-circulating oven is used to simulate control cabinet service, with periodic measurement of retention force on the metal terminal insert on a universal testing machine. UL 94 V-0 cannot be assumed for this unreinforced impact-modified grade; if the panel standard requires V-0, an additional flame-retardant grade or barrier design is necessary.
| Assessment | Standard | Condition or threshold |
|---|---|---|
| Comparative tracking index | IEC 60112 | Solution A, 50 drops without tracking |
| Glow-wire flammability index | IEC 60695-2-12 | 750 °C or 850 °C depending on end product |
| Glow-wire ignition temperature | IEC 60695-2-13 | Report at final wall thickness |
| Insulation coordination | IEC 60664-1 | Pollution degree 2, overvoltage category II/III |
Appliance circulation pump bodies in residential dishwashers expose the polymer to warm detergent solution, mineral scale, and intermittent pressure pulses; VALOX 357X is selected for impeller hubs and pump covers when the alternative glass-filled PBT would create excessive abrasive wear on the shaft seal. The molding process uses two-cavity hot-runner tooling with sequential valve gating to balance fill pressure because the impact modifier increases viscosity in thin impeller blade sections compared with unmodified PBT. Melt temperature is limited to 245 °C and barrel residence time to 5 min maximum to avoid degradation of the impact-modifier phase, which appears as a loss of weld-line strength at the impeller hub rather than as a visible discoloration. The impeller is dimensionally checked after 48 h water immersion at 60 °C per ISO 62, and the shaft insert pull-out force is measured before and after 200 h exposure to a 0.2 % sodium hydroxide solution at 50 °C. Melt volume-flow rate can be checked by ISO 1133-1:2022 at 250 °C with a 2.16 kg load to detect lot-to-lot viscosity shifts before production. Published data for the specific grade in aggressive alkaline dishwasher media is limited, so part validation includes functional pump cycling with hard water at 70 °C to detect stress cracking before the material is approved.
Deicing brines containing 30 % calcium chloride and 5 % magnesium chloride impose a combination of polar liquid absorption and electrochemical stress cracking on roadside sensor enclosures, and 357X is used in these enclosures only after confirming that the housing seal does not trap liquid against a press-fit metal insert. The impact-modifier phase provides low-temperature ductility that survives installation at -25 °C using a percussion driver, which is required for thermoplastic enclosures mounted on steel poles. Injection molding uses a mold temperature of 90 °C to maximize crystallinity and reduce solvent absorption in the amorphous regions, while the melt temperature is held at 250 °C to 255 °C. The enclosure is tested per IEC 60529 IP65 after thermal cycling between -40 °C and 65 °C, and the sealing boss around the cable gland is subjected to a 0.5 N·m torque retention test after 1000 h salt mist exposure per IEC 60068-2-52. Because PBT absorbs less moisture than polyamide but remains susceptible to hydrolysis at elevated temperature and high humidity, the enclosure wall thickness at the thread boss is increased from 2.0 mm to 2.5 mm to compensate for stress relaxation. Published data for 357X in calcium chloride brine immersion is limited, so a direct immersion test at 23 °C and 50 °C for 1000 h is required before approval.
Outdoor LED driver enclosures in cold climates require the housing to absorb impact during ice-clearing strikes without transferring stress to the potting compound, and 357X is processed into a two-shell clamshell with snap-fit closure at melt temperature 250 °C and mold temperature 80 °C. The tool uses a cold runner with a tunnel gate because the enclosure has an internal living hinge for the wiring compartment, and the gate scar is placed on a non-cosmetic surface. Low-temperature notched Izod testing per ISO 180/A at -30 °C is used to qualify the grade after molding because impact-modified PBT may show a transition from ductile to brittle behavior in the range of -20 °C to -40 °C, depending on moisture content. The potting compound, usually a two-part polyurethane, releases exothermic heat during cure, and the enclosure wall must withstand a local temperature of 85 °C for 30 min without distortion; this is verified by a fixture holding the housing at the critical dimple. Creepage and clearance between the AC input terminals and the grounded metal end cap are checked per IEC 60664-1 pollution degree 2, and the comparative tracking index is measured per IEC 60112. Because PBT is susceptible to hydrolysis at high humidity and elevated temperature, outdoor enclosures are limited to applications where the internal temperature does not exceed 65 °C at 80 % relative humidity for continuous service; above this, a polycarbonate or PBT/ASA blend should be evaluated.
Bearing seat geometries in fractional horsepower motor end caps are frequently gated in a way that produces an internal weld line near the bearing cup, and the use of impact-modified PBT requires the mold designer to move the gate to the central sprue or use three point gates to avoid a knit line crossing the bearing load path. The part is molded at 255 °C melt temperature and 90 °C mold temperature, with a packing pressure profile that holds the bearing seat diameter to ±0.05 mm without secondary machining. The end cap is assembled with a sintered bronze bearing by a mechanical insertion process that generates circumferential hoop stress, and the strain at the bearing seat is estimated by a pressure-displacement curve on a servo press. Thermal cycling between -40 °C and 120 °C for 500 cycles is applied to the assembled motor, after which bearing retention force is measured and compared with the 100 N minimum pull-out specification. Because the impact-modifier phase can concentrate near the surface under high shear during filling, the outer skin of the bearing seat may have a slightly different thermal expansion response than the core; this is evaluated by differential scanning calorimetry per ISO 11357 and by cross-sectional microscopy after an annealed 1 h exposure at 120 °C. Published data for 357X in press-fit bearing seats at the upper end of the thermal cycling range is limited, so prototype motors are tested with bearing insertion and removal cycles until the retention force falls below the specification limit.
Competitive SABIC VALOX™ Impact-Modified PBT 357X prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
SABIC VALOX™ Impact-Modified PBT 357X is an unreinforced, impact-modified polybutylene terephthalate injection-molding resin in which a phase-separated elastomeric impact modifier is dispersed in a semicrystalline PBT matrix. The base PBT polymer is produced from 1,4-butanediol and dimethyl terephthalate or terephthalic acid; the impact modifier is not a monomeric plasticizer, and therefore the glass-transition temperature of the continuous PBT phase is not reduced to the extent observed with external plasticization. Published typical values include a density of 1.31 g/cm³ (ISO 1183), a tensile stress at yield of 47 MPa (ISO 527-2/1A), and a tensile elongation at break greater than 50% (ISO 527-2/1A). The flexural modulus is approximately 2000 MPa (ISO 178), which places this product below glass-fiber-reinforced PBT grades in bending stiffness. The notched Izod impact at 23 °C is published as 800 J/m (ASTM D256); ISO notched impact values must be read from the current regional SABIC datasheet because specimen geometry, notch radius, and clamping conditions differ. The material is rated UL 94 HB at 1.5 mm and should not be substituted for flame-retardant grades such as VALOX 310SE0 or VALOX 420SEO without a flame-barrier review. The product is intended for injection molding of clips, snap-fit housings, electrical connectors, and appliance components where crack initiation resistance is more important than high-temperature load retention.
The semicrystalline PBT phase shows a crystalline melting peak in the region of 223 °C when measured by differential scanning calorimetry at 10 K/min (ISO 11357-3). Mold-temperature selection determines the crystalline skin-core morphology. When the mold wall temperature remains below 50 °C, quenched amorphous skins coexist with a slowly cooled crystalline core; differential crystallization shrinkage can produce post-molding distortion after hot-air aging or paint-bake cycles. Annealing at 120 °C for 1 h relaxes some molded-in stress but is not a remedy for inadequate packing. For dimensional stability under ISO 294-4, a mold temperature of 80 °C to 90 °C is preferable for unfilled impact-modified PBT, though it increases cycle time and heat-recovery load.
The principal difference from general-purpose unfilled PBT is notched Izod energy. Standard unfilled PBT grades typically fall below 100 J/m (ASTM D256), whereas the 357X formulation reaches 800 J/m at 23 °C. The impact modifier dissipates energy through shear yielding and cavitation at the notch tip; the notch-sensitive crack propagation mode of the unmodified polyester is suppressed. The increase is not linear with modifier concentration, and excessive impact-modifier addition can reduce tensile yield stress and create delamination at knit lines. Compared with 30% glass-fiber-reinforced VALOX 420SEO, 357X trades flexural modulus and heat deflection temperature for tensile elongation. A 30% glass-filled PBT grade typically presents a tensile modulus near 9000 MPa (ISO 527-2/1A) and an HDT/A above 200 °C (ISO 75-2/Af); the unfilled impact-modified grade remains near 2000 MPa and 55 °C under the same HDT/A load. The structural difference is clear: 357X is a ductile, low-stiffness material for snap-fit and impact-limited designs, while glass-filled VALOX grades are selected for dimensional stability and load-bearing capability at elevated temperature. Compared with flame-retardant unfilled PBT, 357X does not carry a V-0 classification; flame-retardant grades commonly sacrifice some impact resistance to meet vertical burn requirements.
Desiccant drying is required before melt processing because the polyester linkage is hydrolytically sensitive. Above 200 °C, water attacks the ester groups and reduces molecular weight; the degradation is irreversible and can be measured as a loss in intrinsic viscosity by dilute-solution viscometry (ISO 1628-5). A practical drying boundary is 4 h at 120 °C in a closed-loop desiccant dryer with a return-air dew point no higher than -30 °C. When ambient relative humidity exceeds 60%, open hopper loading must be replaced by direct feed from the dryer shut-off station or a nitrogen-purged hopper to prevent moisture regain. Retention below 0.02 wt% moisture by Karl Fischer titration is the boundary stated in SABIC processing guidance for PBT. Melt temperature should remain between 245 °C and 260 °C; mold temperature should remain between 60 °C and 90 °C for most unfilled impact-modified PBT applications. Production-scale screw geometry of 20:1 to 24:1 L/D with a compression ratio of 2.5:1 to 3.5:1 is standard for unfilled PBT. Regrind levels above 25 wt% may widen notched Izod scatter because repeated heat history degrades the impact-modifier domain; process capability studies should validate the upper regrind fraction for each tool.
Rheological characterization of unfilled impact-modified PBT shows shear-thinning behavior typical of a pseudoplastic melt. Capillary rheometry at 250 °C records a flow index below 1; at shear rates above 1000 s⁻¹, apparent viscosity may fall by more than half relative to low-shear values. This permits filling of thin ribs and long flow paths but also makes gate-velocity selection critical. In valve-gated multicavity tools, sequential opening delayed beyond 1.5 s can freeze the gate at mold temperatures below 60 °C and produce short shots. The elastic character of the impact-modifier phase contributes to die swell and can promote jetting if the gate is too small for the shot volume. Excessively long gate lands increase shear heating; very short lands produce unstable gate freeze-off. For multicavity tools, runner balancing should be based on pressure-drop calculation rather than geometric symmetry alone because the impact-modified melt does not behave as a simple Newtonian fluid under low-pressure filling.
| Property | Standard / Method | Published Typical Value | Test Condition |
|---|---|---|---|
| Density | ISO 1183 | 1.31 g/cm³ | 23 °C |
| Tensile stress at yield | ISO 527-2/1A | 47 MPa | 5 mm/min |
| Tensile elongation at break | ISO 527-2/1A | >50% | 5 mm/min |
| Flexural modulus | ISO 178 | 2000 MPa | 2 mm/min |
| Notched Izod impact | ASTM D256 | 800 J/m | 23 °C |
| Heat deflection temperature, HDT/A | ISO 75-2/Af | 55 °C | 1.8 MPa |
| Mold shrinkage, flow | ISO 294-4 | 0.020–0.026 cm/cm | Optimized molding |
| Flammability | UL 94 | HB | 1.5 mm |
At -40 °C, impact-modified PBT grades typically show a sharp drop in notched Izod because the elastomer phase approaches or falls below its glass transition. The published room-temperature value of 800 J/m is therefore not sufficient for cold-start underhood qualification; end users must request low-temperature notched Izod data or generate their own per ASTM D256 or ISO 180/1A on conditioned specimens. The HDT/A of 55 °C defines another boundary: continuous load-bearing service above this temperature is not appropriate, and glass-filled or mineral-filled grades should be substituted if dimensional stability under load is required above 120 °C. The UL 94 HB rating at 1.5 mm is a horizontal burn classification. Electrical or electronic enclosures requiring V-0 must not be qualified with this product unless additional flame-retardant barriers or a different SABIC grade are used.
Part design using 357X should avoid sharp corners in load paths. A minimum fillet radius of 0.5 mm reduces stress concentration and prevents notch effect in impact loading. For snap-fit beams, the allowable strain should be selected below the tensile strain at break because molded-in stress and weld lines consume part of the available elongation. Strain recovery after repeated snap-fit cycling is time-dependent; at elevated temperatures above 60 °C, creep can reduce retention force. The product should not be used in constant-load springs without creep testing under ISO 899-1 or equivalent. Ejector pins should be large and well polished; sharp transitions in ejection can whiten impact-modified surfaces due to craze formation under tensile ejection stress. Textured surfaces require draft angles above 1.5° to prevent scuffing. Vent depths of 0.02 mm to 0.03 mm are typical for unfilled PBT; blocked vents produce gas burn and inhibit crystallinity at the flow front.
In production-scale injection molding, high shear in narrow gates and thin walls can raise melt temperature above the set barrel profile. At 260 °C, melt residence time should be kept below 5 min; beyond this boundary, ester cleavage and tetrahydrofuran evolution produce a measurable viscosity loss and discoloration. Hot-runner manifolds with stagnant zones are a common failure source because a fraction of the melt can remain at temperature for several cycles. The machine shot size should consume at least 50% of barrel capacity per cycle, and screw decompression should be limited to 2 mm to 3 mm to reduce air entrapment. Switching from polycarbonate to PBT without purging can generate transesterification products at the interface; a dedicated PBT purge or a low-viscosity purging compound should be used. Weld lines in double-gated tools remain property troughs even in impact-modified PBT. The impact modifier improves weld-line integrity relative to unmodified PBT, but tensile elongation at break under ISO 527-2/1A is still lower at knit lines than in single-gate controls. Mold temperatures below 60 °C tend to sharpen visible weld-line boundaries and reduce local impact resistance.
Compliance claims are lot-specific and regional. The product is generally formulated to comply with RoHS 2011/65/EU and delegated amendment (EU) 2015/863, but absence of restricted substances must be confirmed against the current SABIC product stewardship declaration. REACH SVHC content must be evaluated at the article level; the typical threshold above 0.1 wt% triggers communication obligations. No unconditional food-contact or medical-clearance statement applies to all colors, production sites, and processing aids. The grade is not recommended for continuous exposure to hot amines, strong alkalis, or aqueous glycol systems above 80 °C without end-use chemical compatibility testing; stress cracking in PBT can occur in amine-containing coolants under molded-in strain. The UL 94 HB classification is valid only at the specified 1.5 mm thickness and should not be extrapolated to thinner sections.
| Requirement | Standard / Regulation | Published Classification | Verification Requirement |
|---|---|---|---|
| Flammability | UL 94 | HB at 1.5 mm | UL yellow card |
| Heavy metals and flame retardants | RoHS 2011/65/EU, (EU) 2015/863 | Generally compliant | Lot-specific SABIC declaration |
| SVHC communication | REACH EC 1907/2006 | No reportable content above 0.1 wt% | Article-specific review |
| Food contact | FDA 21 CFR, EU 10/2011 | Not unconditional | Migration testing required |
The compliance table is not a substitute for the SABIC product stewardship file. Color concentrates, regrind, and external processing aids can alter the article-level regulatory profile. For applications involving continuous outdoor exposure, UV stabilization must be specified; the standard 357X grade may not contain a sufficient UV package for long-term weathering under ISO 4892-2 or ASTM G154. For black or custom colors, carbon black can provide UV absorption but may increase mold shrinkage by nucleating crystallization; shrinkage verification under ISO 294-4 is then mandatory for precision fits.
Application placement for SABIC VALOX 357X includes unfilled clip bodies, terminal retainers, power-tool housings, and appliance latch mechanisms where drop-impact resistance is required. For terminal retainers, the high notched Izod reduces insertion cracking, but the HDT/A of 55 °C excludes continuous engine-compartment header seating. Connector bodies molded from 357X provide more ductile snap-fit behavior than glass-filled PBT but less dimensional precision; tool shrinkage studies under ISO 294-4 are required for multicavity conversion. In fuel or oil exposure combined with impact loading, published data for this specific configuration is limited; qualification should include property retention after fluid immersion under ISO 1817 or customer-specific equivalents. Selection between standard unfilled PBT, impact-modified PBT, and glass-filled PBT therefore remains an application-specific trade-off based on notched Izod, flexural modulus, HDT/A, and flame classification.