| HS Code | 225590 |
| Polymer Type | High Density Polyethylene |
| Density | 0.954 g/cm³ |
| Melt Flow Index | 0.35 g/10 min at 190°C/2.16 kg |
| Tensile Strength At Yield | 26 MPa |
| Elongation At Break | 800 % |
| Flexural Modulus | 1200 MPa |
| Vicat Softening Temperature | 124 °C |
| Melting Temperature | 131 °C |
| Environmental Stress Crack Resistance | >1000 h |
| Shore D Hardness | 65 |
| Water Absorption | <0.01 % |
| Dielectric Constant | 2.3 |
| Volume Resistivity | >1e16 ohm·cm |
| Thermal Conductivity | 0.45 W/m·K |
As an accredited Reliance Industries HDPE HD5301AA factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Reliance Industries HDPE HD5301AA is typically supplied in 25 kg polyethylene bags, palletized, stretch-wrapped, and labeled for industrial transport. |
| Container Loading (20′ FCL) | 20′ FCL container loaded with Reliance Industries HDPE HD5301AA in 25kg bags, palletized, shrink-wrapped, securely braced for safe ocean shipment. |
| Shipping | Reliance Industries HDPE HD5301AA is shipped as non-hazardous polyethylene pellets, not regulated for transport. Standard packaging includes 25 kg PP woven bags, palletized and stretch-wrapped, or bulk bags/containers. Transport in clean, dry vehicles and store cool, dry, ventilated, away from direct sunlight, heat, and moisture. Handle with standard industrial precautions. |
| Storage | Store Reliance Industries HDPE HD5301AA in a cool, dry, well-ventilated area, away from direct sunlight, heat, flames, and oxidizing agents. Keep original packaging closed to prevent moisture, dust, and contamination. Avoid prolonged UV exposure and extreme temperatures. Stack pallets securely and avoid damaging bags. Observe good housekeeping and follow the safety data sheet and local regulations. |
| Shelf Life | Reliance HDPE HD5301AA typically has a 24-month shelf life if stored cool, dry, away from direct sunlight in original packaging. |
Blown film conversion of HD5301AA on a 90 mm single-screw extruder with L/D 30:1 barrier screw and 250 mm spiral mandrel die is normally run at 80–120 kg/h, 195–210 °C melt temperature, and 3.0–3.5:1 blow-up ratio. Frost line height is held at 500–700 mm. Under these conditions 12–20 μm film retains a balance between machine-direction tear resistance and transverse-direction tensile strength. The formulation for retail carrier bag film does not exceed 5 wt% C6-LLDPE because at 5 wt% laboratory evaluation according to ASTM D882-18 shows transverse-direction tensile strength of 28–32 MPa, while dart impact according to ASTM D1709-16a Method A shifts from 90–120 g for neat HD5301AA to 130–170 g for the blend. Tear resistance is assessed according to ASTM D1922-15; the machine-direction/transverse-direction tear ratio remains above 1.8:1 when frost line height is below 700 mm. Production-scale failure modes include bubble oscillation and melt fracture at die shear rates above 450 s⁻¹, observed as rough inner bubble surface and gauge bands. If melt temperature falls below 190 °C, die pressure increases by 12–18 % and film width variability exceeds ±3 mm; if melt temperature exceeds 220 °C, oxidation generates gel particles detectable as optical defects under ASTM D1003-13 haze testing. For food-contact carrier bags, the grade must be certified under FDA 21 CFR 177.1520(c) subsection 3.1a and Regulation (EU) No 10/2011 with overall migration below 10 mg/dm².
High-stalk film lines processing HD5301AA operate within a narrower envelope than low-stalk lines because the high melt viscosity of the 0.30–0.50 g/10 min melt index band produces elevated extensional stress in the stalk. On a 120 mm extruder with a 400 mm die, die gap 1.2–1.6 mm, and blow-up ratio 4.0–5.0:1, the bubble is suspended 800–1,100 mm above the die before frost line. Melt temperature is restricted to 200–215 °C; operation below 200 °C raises die pressure to 320–360 bar and initiates sharkskin melt fracture, while operation above 215 °C thins the stalk and produces breathing marks. Cooling air velocity at the stabiliser is set at 6–10 m/s. The process yields tubular film for heavy shopping bags and industrial liners in the 20–30 μm thickness range. Under these conditions, tensile properties measured according to ISO 527-3:2018 are typically 45–55 MPa in machine direction and 30–38 MPa in transverse direction. Dart drop measured according to ASTM D1709-16a Method B for 25 μm film stays in the 180–240 g range. A practical limitation is batch-to-batch melt index variation of ±0.05 g/10 min; this variation shifts die pressure by 10–14 % and changes frost line height by 80–120 mm at constant output. The table below records the comparative envelopes used on production-scale low-stalk and high-stalk lines.
| Processing variable | Low-stalk carrier film | High-stalk film |
|---|---|---|
| Melt temperature | 195–210 °C | 200–215 °C |
| Die gap | 1.8–2.0 mm | 1.2–1.6 mm |
| Blow-up ratio | 3.0–3.5:1 | 4.0–5.0:1 |
| Frost line height | 500–700 mm | 800–1,100 mm |
| Cooling air velocity | 4–6 m/s | 6–10 m/s |
Accumulator-head extrusion blow moulding of HD5301AA for 10–30 L industrial containers and jerry cans requires a melt temperature of 180–200 °C, blow pressure 0.6–0.8 MPa, and mould temperature 15–30 °C. The formulation is neat HD5301AA with 1.0–1.5 wt% carbon black masterbatch containing 40 wt% carbon black in an LLDPE carrier; the carbon black content in the finished wall is therefore 0.4–0.6 wt%. Screw speed on a 100 mm extruder with L/D 24:1 and grooved feed section is limited to 30–50 rpm. Parison sag becomes significant above 205 °C when shot mass exceeds 2.5 kg, producing wall-thickness variation above ±12 % and top-load failure in the shoulder region. Finished containers are tested according to ASTM D2463-15 for drop impact at -20 °C and according to ASTM D1693-15 Condition B for environmental stress crack resistance; F50 values above 500 h are accepted for moderate-risk liquids. Stack load testing is performed according to ISO 2234:2015 at 40 °C for 24 h, with creep deformation below 3 mm. Flash control at the parting line requires mould clamping force of 60–120 t for a 15 L jerry can. Regrind addition above 20 wt% reduces ESCR F50 from above 500 h to below 300 h and increases surface roughness at the pinch-off weld.
In heavy-duty industrial liner conversion, plant regrind is introduced at 15–25 wt% into virgin HD5301AA only after regrind from edge trim and rejected film has been densified and screened to remove particles larger than 1.5 mm. Extrusion on a 120 mm single-screw line with L/D 30:1, 400 mm annular die, 2.0 mm die gap, and 3.0:1 blow-up ratio produces 75–150 μm film at 180–210 °C melt temperature. The formulation adds 0.5–1.0 wt% hindered phenolic antioxidant masterbatch and 0.3–0.5 wt% slip/antiblock masterbatch based on erucamide and synthetic silica; the silica loading in the finished film remains below 1,500 ppm to preserve Elmendorf tear resistance. Tensile properties are checked according to ISO 527-3:2018, puncture resistance according to ASTM D5748-19, and slow crack growth resistance according to ISO 16770:2004 at 50 °C. On production lines, regrind addition above 25 wt% lowers ESCR F50 from above 500 h to below 200 h and increases gel count by 30–50 % under ASTM D1003-13 haze evaluation. The finished article is used as construction debris sacks, agricultural silage covers, and temporary containment liners; when intended for chemical contact, the liner is not used for hydrocarbons because swelling exceeds 3 % mass gain after 72 h immersion in toluene at 23 °C according to ISO 175:2010. Pre-drying is not normally required, but after storage at relative humidity above 60 %, surface moisture is removed at 70–80 °C for 2–4 h in a desiccant dryer with dew point -30 °C.
Flat-die extrusion of HD5301AA for geomembrane sheet is carried out on a 150 mm single-screw extruder with L/D 30:1, a 2,000 mm coat-hanger die, and a three-roll polishing stack set at 50–70 °C. Melt temperature is controlled at 200–215 °C; sheet thickness ranges from 1.0 mm to 2.5 mm. Carbon black masterbatch with 50 wt% carbon black in HDPE carrier is added at 2.0–2.5 wt% to achieve finished carbon black content of 1.0–1.25 wt%. Above 2.5 wt% masterbatch, dispersion quality measured according to ISO 18553:2002 degrades: fused agglomerates larger than 60 μm appear, and dart puncture resistance according to ASTM D4833-07 declines by 15–25 % relative to 2.0 wt% loading. The stabiliser package consists of 0.2–0.5 wt% HALS masterbatch and 0.1–0.3 wt% hindered phenolic/phosphite antioxidant masterbatch; oxidative induction time measured at 200 °C according to ISO 11357-6:2018 is maintained above 25 min. Weldability is evaluated by hot-wedge welding at 320–370 °C wedge temperature and 2.0–3.0 m/min weld speed; peel separation in shear mode must remain below 10 % of the welded seam area. The compliance matrix for geomembrane applications is provided below. Published data for HD5301AA at carbon black loadings above 2.5 wt% in flat-die sheet is limited; the boundary is derived from production-scale HDPE sheet lines with equivalent melt index and density.
| Requirement | Standard or regulation | Measurement condition / limit |
|---|---|---|
| Density | ASTM D1505-18 | 0.952–0.956 g/cm³ |
| Melt flow rate | ISO 1133-1:2022 | 190 °C / 5 kg, 0.30–0.50 g/10 min |
| Environmental stress crack resistance | ASTM D1693-15 Condition B | 10% Igepal, 50 °C, F50 > 500 h |
| Oxidative induction time | ISO 11357-6:2018 | 200 °C, OIT > 25 min |
| Carbon black dispersion | ISO 18553:2002 | Agglomerate size < 60 μm |
| REACH SVHC | Regulation (EC) No 1907/2006 | < 0.1 wt% |
| RoHS restricted substances | Directive 2011/65/EU Annex II | Pb, Hg, Cd, Cr(VI), PBB, PBDE limits |
Because low melt index raises die pressure, tape lines feeding HD5301AA are configured with a 65 mm single-screw extruder with L/D 30:1, a flat film die gap of 0.5–0.8 mm, and a water bath at 30–45 °C. The formulation uses neat HD5301AA with 2–4 wt% coloured masterbatch and 0.2–0.5 wt% polyolefin processing aid; filler or calcium carbonate is excluded because it increases draw resonance at draw ratios above 6:1. The quenched primary tape is slit and orientated at 5:1–8:1 draw ratio in a hot-air oven set at 110–130 °C, followed by annealing at 80–110 °C on heated godets. At take-off velocities below 120 m/min, final tape tensile strength according to ISO 527-2:2012 is 280–350 MPa in the orientation direction, with elongation at break 15–25 %. Above 180 m/min, tape fibrillation and edge splitting are observed when the draw ratio exceeds 8:1; this failure is measured as a reduction in tape tenacity from 4.5–5.5 cN/dtex to below 3.5 cN/dtex. The woven fabric is tested for UV resistance according to ASTM G154-16 Cycle 2 for 500 h; tensile retention must be above 70 %. Finished articles include woven sacks, flexible intermediate bulk container fabrics, and tarpaulins.
Sheet extrusion of HD5301AA for reusable logistics trays uses a 120 mm extruder with L/D 30:1, a 1,500 mm flat die, and a three-roll stack with roll temperatures of 40–60 °C. Sheet thickness is maintained at 1.5–3.0 mm with thickness tolerance ±5 %; recycled sheet from skeletal scrap is reintroduced at 30–50 wt% without antioxidant top-up if the regrind fraction has been processed for no more than three heat histories. Thermoforming is performed on a plug-assist pressure former with sheet surface temperature 165–180 °C, mould temperature 40–60 °C, forming pressure 0.4–0.6 MPa, and cycle time 20–35 s. Wall thickness distribution is checked by ultrasonic thickness gauge; corner thinning below 40 % of nominal sheet thickness is rejected because drop impact failure occurs at -20 °C according to ISO 6603-2:2019. Flexural modulus of the formed tray is measured according to ISO 178:2019; values of 1,100–1,300 MPa are typical. The trays are used for automotive component dunnage and industrial material handling; the grade is not suitable for direct contact with oily metal parts unless a barrier liner is used because oil absorption causes surface swelling of 1.5–2.5 % after 168 h at 23 °C according to ISO 175:2010. Process failure modes on production lines include sheet sag in the preheater when surface temperature exceeds 180 °C, and corner thinning when plug speed exceeds 200 mm/s.
Competitive Reliance Industries HDPE HD5301AA prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Reliance Industries HDPE HD5301AA is a high-molecular-weight high-density polyethylene blow moulding resin based on a bimodal molar mass distribution. The grade is specified for extrusion blow moulding of large-volume containers, automotive fuel tanks, and industrial packaging where environmental stress crack resistance and parison stability are required. Under ASTM D1238 at 190 °C with a 5 kg load, the typical melt flow rate is 0.35 g/10 min, while the 21.6 kg melt flow rate is typically 5.5 g/10 min. The resulting flow-rate ratio of 15.7 is characteristic of a broadly distributed high-molecular-weight polyethylene with pronounced shear thinning. Density determined by ASTM D1505 falls within the 0.950 g/cm³ to 0.956 g/cm³ range in published lot-release data. Tensile yield stress measured at 23 °C using ISO 527-2 is typically 27 MPa, and elongation at break exceeds 600 %. Flexural modulus under ISO 178 is approximately 1100 MPa.
| Property | Standard | Typical value/range |
|---|---|---|
| Melt flow rate 190 °C/5 kg | ASTM D1238 | 0.35 g/10 min |
| Melt flow rate 190 °C/21.6 kg | ISO 1133-1:2022 | 5.5 g/10 min |
| Density | ASTM D1505 | 0.950–0.956 g/cm³ |
| Tensile yield stress | ISO 527-2 | 27 MPa |
| Elongation at break | ISO 527-2 | 600 % minimum |
| Flexural modulus | ISO 178 | 1100 MPa |
| ESCR F50, Condition B, 100% Igepal CO-630, 50 °C | ASTM D1693-15 | 600 h minimum |
| Vicat softening temperature A50 | ISO 306 | 124 °C |
The bimodal molar mass distribution generates two distinct rheological populations. The lower-molar-mass fraction lowers the high-shear viscosity during extrusion through the die, while the high-molar-mass fraction increases zero-shear viscosity and melt strength during parison formation. This distribution is not equivalent to a simple broadened unimodal distribution; it is designed to preserve shear thinning at the high apparent shear rates encountered in accumulator-head tooling while limiting parison sag. Under ISO 1133-1:2022, the ratio of the 21.6 kg melt flow rate to the 5 kg melt flow rate is approximately 15.7, whereas many narrow-distribution blow moulding grades exhibit ratios in the 8 to 12 range. The difference in flow-rate ratio affects die swell, head-pressure build-up, and wall-thickness programming. Published constitutive viscosity data for this specific grade is limited; capillary rheometry under ISO 11443 at 190 °C would be required to quantify the shear-viscosity curve for a given lot.
The high-molar-mass fraction also controls slow crack growth resistance through tie-chain and entanglement density. In practice, this means that processor adjustments cannot compensate for loss of the high-molar-mass fraction; overheating above 240 °C can degrade that fraction selectively through oxidative scission, reducing ESCR before any visible discoloration. On production lines with accumulator-head machines, this degradation has been observed as a progressive reduction in parison hang time at constant melt temperature and die gap, followed by an increase in drop-impact failures in moulded drums. Therefore, melt-temperature management is as important as moisture control for retaining the grade’s design properties.
On accumulator-head machines with screw L/D ratios of 24:1 to 30:1, the resin is typically processed at barrel temperature zones from 170 °C in the feed to 205 °C in the metering section, with head and die temperatures held between 200 °C and 210 °C. Melt temperature above 240 °C should be avoided because oxidative chain scission and gel formation increase; below 180 °C, melt fracture and head-pressure fluctuations become more frequent on grooved-barrel extruders. Pre-drying is normally unnecessary at granulate surface moisture levels below 0.05 wt%, but condensation at RH above 60 % can produce surface splay in the parison.
Accumulator-head equipment requires screw geometries capable of generating high melt homogeneity at low melt index. Barrier screws with a Maddock mixer or static melt mixers are commonly used; their L/D ratios are typically between 24:1 and 30:1. The high-molar-mass fraction of HD5301AA produces measurable die swell, which is controlled by die gap adjustment and parison programming. A starting die gap of 2 mm to 4 mm is used in many large-container tools, but final gap settings depend on shot size, clamp stroke, and container wall geometry. Parison sag is not a simple function of melt flow rate alone; the zero-shear viscosity of the high-molecular-weight fraction retards sag during the parison drop phase. No universal parison sag value can be assigned because sag is governed by local melt temperature, die gap, shot mass, and drop time. Published data for this specific configuration is limited; however, production trials on shuttle machines with 2.5 kg to 10 kg shots indicate that die-temperature uniformity and clean die lips are required to avoid localized thinning and weld-line displacement.
Wall-thickness programming is essential when converting from lower molecular weight grades. Because HD5301AA retains more melt strength, the parison may not elongate as rapidly under its own weight. Operators have been observed compensating by raising head temperatures above 220 °C; this practice reduces the high-molar-mass contribution and should be replaced with die-gap and servo-parison profile changes. In accumulator-head machines, the shot-accumulation time should be kept below the residence-time limit of the high-molecular-weight fraction; prolonged hold times above 200 °C can increase gel formation.
Environmental stress crack resistance is the primary technical differentiator for HD5301AA in chemical drum and fuel tank service. Under ASTM D1693-15 Condition B with 100 % Igepal CO-630 at 50 °C, the failure time for 50 % of specimens is reported above 600 h. The property is attributed to the high molar mass fraction, which generates tie-chain and chain-entanglement density that retards slow crack growth in the presence of polar surfactants and hydrocarbon permeates. In contrast, conventional unimodal HDPE grades with density above 0.960 g/cm³ can exhibit significantly shorter F50 values under the same test, often below 100 h. For a 210 L chemical drum, this difference is operationally relevant: the drum wall is continuously exposed to internal stress from hydrostatic pressure and external stress from clamp handling, while aggressive liquids can act as stress-cracking agents. Slow crack growth resistance is not captured by density or melt index alone; it requires ESCR testing on notched specimens or full-container stacking tests.
Changing from a conventional unimodal HDPE of density 0.958 g/cm³ or higher to HD5301AA changes both the extrusion and the performance testing envelope. The lower density of HD5301AA reduces top-load stiffness relative to high-density unimodal grades; therefore stacking performance under ISO 12048 must be re-evaluated rather than assumed from material density alone. Drop impact resistance after conditioning at -18 °C is typically improved because the high-molar-mass fraction raises impact toughness. In UN dangerous goods certification, drop heights are assigned by packing group: 1.8 m for packing group I, 1.2 m for packing group II, and 0.8 m for packing group III. Container designers selecting HD5301AA for hazardous liquids should therefore conduct drop tests on the moulded drum at the specific packaging group requirement, because processing-induced wall-thickness variation rather than resin properties alone controls the failure mode.
Extruder power demand can increase during changeover. The high-molecular-weight fraction raises head pressure, especially at high parison drop speeds. Accumulator-head machines with undersized hydraulic drives may show reduced shot capacity if the die gap is not opened or if the melt temperature is too low. In practice, a screw speed reduction of 10 % to 20 % may be required during the transition until torque stabilizes. This is a production-scale observation on continuous shuttle blow moulding lines, not a resin defect; the condition resolves with appropriate barrel temperature flattening and flow channel geometry.
In automotive fuel tank production, HD5301AA is not used as a monolayer material where stringent hydrocarbon permeation limits apply; instead it functions as the high-molecular-weight HDPE skin layer in coextruded six-layer barrier structures containing an ethylene-vinyl alcohol barrier layer and maleic anhydride-grafted tie resin. Permeation requirements under CARB LEV III, EPA Tier 3, and Euro 6 are met by the barrier layer, while HD5301AA contributes low-temperature impact and slow crack growth resistance. Adhesion between HD5301AA and unmodified EVOH is insufficient in production; maleated polyolefin tie layers are required. Rheological matching of the skin and barrier layers is critical to prevent interfacial instability, particularly at the die swell ratios of the HDPE skin. Fuel tank drop-impact validation under UN ECE R34 Annex 5 and equivalent vehicle manufacturer specifications is performed on finished tanks, because weld regions and pinch-off zones are controlled by tooling, coextrusion layer distribution, and parison programming rather than by the skin resin alone.
The grade differs from injection moulding HDPE primarily in its 5 kg melt flow rate of 0.35 g/10 min, which makes thin-wall injection moulding impractical because melt viscosity at high shear remains high enough to create excessive pressure drop in runner systems and freeze-off at the gate. Compared with PE100 pipe grades, HD5301AA is not designed for pressure piping service under ISO 9080 or ISO 12162; it lacks the long-term hydrostatic strength classification associated with pipe-grade HDPE. Compared with standard blow moulding HDPE of density 0.958 g/cm³ to 0.964 g/cm³, HD5301AA provides longer ESCR under ASTM D1693-15 Condition B but lower top-load stiffness. For 20 L to 30 L containers requiring maximal rigidity at ambient and elevated temperatures, a higher-density unimodal grade may be more appropriate if ESCR demands are moderate.
The resin can be evaluated under FDA 21 CFR 177.1520 for olefin polymers in food-contact applications, and a conforming lot may be supported by EU 10/2011 migration test declarations for specific food simulants. Raw-pellet REACH registration under EC 1907/2006 applies, and RoHS 2011/65/EU heavy-metal limitations apply to homogeneous materials in electrical and electronic equipment, not to the raw resin as supplied. Downstream incorporation of colour concentrates or processing aids alters the regulatory compliance profile; such changes must be validated on the final article. Chemical resistance is broad for a high-density polyethylene: the polymer is attacked by strong oxidizing acids, long-chain aliphatic hydrocarbons can be absorbed, and some surfactant systems accelerate environmental stress cracking. The resin is not recommended for continuous service above 60 °C with strong oxidizing agents, nor for direct contact with aromatic solvents under sustained stress. In multi-layer structures, direct contact with unmodified polyamide or EVOH without tie resin can produce delamination failures on moulded parts.
The grade is supplied with a stabilization package intended for extrusion blow moulding at melt temperatures below 240 °C. Long residence times above this limit consume hindered phenolic antioxidants; the oxidation induction time determined under ISO 11357-6 declines as a function of processing history. Production lots should not be dry-blended with pro-oxidant-containing regrind unless the final article is tested for long-term thermal stability. Published data for this specific configuration is limited; regrind addition levels must be validated by full-container performance tests rather than resin data alone.
| Requirement | Standard/Regulation | Applicability |
|---|---|---|
| Food-contact olefin polymer | FDA 21 CFR 177.1520 | Raw resin subject to final article testing |
| Plastic food-contact material | EU 10/2011 | Migration limits for specific simulants |
| REACH registration | EC 1907/2006 | Substance/imported pellet compliance |
| RoHS heavy metals | 2011/65/EU | Finished EEE article, not raw pellet |
| Plastic fuel tank approval | UN ECE R34 Annex 5 | Finished tank drop and fire performance |
| Melt flow rate | ISO 1133-1:2022 | Incoming QC at 190 °C/21.6 kg |
| ESCR | ASTM D1693-15 Condition B | 100% Igepal at 50 °C |
Incoming quality control on a production line should include melt flow ratio, density, and ESCR as lot-release checks. Melt flow rate is determined on dried samples under ISO 1133-1:2022; density is measured on compression-moulded plaques conditioned for 24 h at 23 °C according to ISO 1183-1. FTIR analysis of the pellet surface can detect oxidized gel contamination, and grey-scale image analysis of pressed films can quantify gel counts above 200 µm. Batch-to-batch variation in the 5 kg melt flow rate beyond ±0.03 g/10 min can shift parison sag time on accumulator machines and should trigger die gap adjustment. Material that has been stored in open silos at humidity above 60 % or with wide temperature cycling should be sampled for surface moisture before entering the extruder feed throat, because surface condensation rather than core pellet moisture is the more common cause of parison pitting on automated lines.