Ravago Hdpe Rpehd

Ravago HDPE RPEHD

    • Product Name: Ravago HDPE RPEHD
    • Factroy Site: Yinchuan, Ningxia, China
    • Price Inquiry: sales8@ascent-chem.com
    • Manufacturer: Ascent Petrochem Holdings Co., Limited
    • CONTACT NOW
    VTB
    Specifications
    HS Code 440327
    Grade Ravago HDPE RPEHD
    Polymertype High Density Polyethylene
    Recycledcontent Yes
    Density 0.955 g/cm³
    Meltflowrate 0.30 g/10 min at 190°C/2.16 kg
    Tensilestrengthatyield 25 MPa
    Tensileelongationatbreak 600%
    Flexuralmodulus 1200 MPa
    Notchedizodimpact 80 J/m
    Heatdeflectiontemperature 75°C at 0.45 MPa
    Vicatsofteningtemperature 125°C
    Shoredhardness 65
    Waterabsorption <0.01%
    Meltingtemperature 130°C
    Moldingshrinkage 0.020 cm/cm

    As an accredited Ravago HDPE RPEHD factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.

    Packing & Storage
    Packing Ravago HDPE RPEHD packaging: 25 kg polyethylene bags, stacked on pallets and wrapped, suitable for industrial handling and storage.
    Container Loading (20′ FCL) 20′ FCL container loaded with Ravago HDPE RPEHD resin in palletized bags, securely stowed for safe ocean transport.
    Shipping Ravago HDPE RPEHD is a non-hazardous polyethylene resin. It is not regulated for transport by DOT, IMDG, or IATA; no UN number, hazard class, or packing group. Ship palletized in sealed bags, sacks, or octabins. Keep dry, cool, and away from contamination. Standard industrial handling applies.
    Storage Always store Ravago HDPE RPEHD indoors in a cool, dry, well-ventilated area, away from direct sunlight, heat, flames, and ignition sources. Keep original containers or bags sealed and palletized, off the floor, to prevent moisture, dust, and contamination. Avoid prolonged UV exposure and contact with incompatible chemicals. Follow all local regulations and the supplier’s SDS for safe handling and storage.
    Shelf Life Ravago HDPE RPEHD typically has no defined shelf life; it remains stable when stored cool, dry, away from sunlight and ignition sources.
    Application of Ravago HDPE RPEHD

    On an accumulator-head extrusion blow molding line with a 120 mm grooved-feed extruder and 25:1 L/D screw, Ravago HDPE RPEHD is processed within a melt temperature corridor of 180 °C to 210 °C. Head pressure is held between 18 MPa and 28 MPa; parison programming must compensate for die swell coefficients of 1.6 to 2.1, measured on the accumulator drop stroke. When post-consumer reclaim is present, melt filtration through 150 µm to 250 µm screen packs upstream of the die head is required to prevent fault lines in the pinched-off tail flash. Clamp force for a 60 L jerrycan mold is typically 400–600 kN; for a 200 L drum stack mold, the clamp requirement rises to 1,500–2,000 kN. Wall thickness is managed with a 100-point parison programmer, and wall thickness variation above ±0.2 mm in the chime region reduces drop impact at −18 °C by more than 30% in production audits. Material entering this application is controlled by melt flow rate per ISO 1133-1:2022 at 190 °C/2.16 kg, density per ISO 1183-1:2019, and environmental stress-crack resistance per ASTM D1693-15. For UN-certified packaging, filled container drop tests per ASTM D5276-19 at 1.8 m and leak testing under 20 kPa internal pressure are used to verify the finished drum.

    Accumulator cycle times for 60 L jerrycans usually run 55–70 s; for 200 L drums, cycle time extends to 120–150 s. Trimmed flash regrind is reintroduced at 30–50 wt% only after lot homogenization because a melt flow rate drift of ±0.2 g/10 min changes parison sag and pinch weld thickness. The resin should be pre-dried at 80 °C for 2–4 h when surface moisture exceeds 0.1 wt% after exposure to 60% RH or higher. Oxidative induction time per ISO 11357-6:2018 at 200 °C in oxygen should remain above 20 min; lower values are associated with pinholes at the pinch seam and early brittle failure in drop tests.

    Control areaStandard designationIndustrial acceptance window
    Melt mass-flow rateISO 1133-1:2022, 190 °C / 2.16 kg0.30–0.55 g/10 min
    DensityISO 1183-1:20190.945–0.960 g/cm³
    Environmental stress-crack resistanceASTM D1693-15, Type B, 10% Igepal, 50 °C> 50 h to F50
    Oxidative induction timeISO 11357-6:2018, 200 °C, O2> 20 min
    Loaded container dropASTM D5276-191.8 m flat drop, 23 °C, no leakage after 3 drops
    Food contact and migrationFDA 21 CFR 177.1520(c), EU 10/2011overall migration < 10 mg/dm²

    What Limits Backpressure Stability During Corrugated Drainage Pipe Extrusion?

    Annular corrugated drainage pipe is produced from Ravago HDPE RPEHD on vacuum-forming corrugators coupled to 75 mm to 90 mm grooved-feed single-screw extruders with 38:1 L/D barrel sections. The melt exits a spiral mandrel pipe die at 200–220 °C and is pinned into mold blocks by differential air pressure of −20 kPa to −60 kPa. Backpressure stability within ±0.8 MPa is critical because corrugator block speed, vacuum level, and die gap interact; when backpressure exceeds ±1.2 MPa, wall thickness in the valley of the corrugation drops below 0.8 mm and ring stiffness falls below the SN8 classification. Polypropylene contamination from mixed municipal bales must be limited to 2–5 wt%, because polypropylene forms unmelted domains that appear as inner-wall blisters and reduce pipe impact toughness under ISO 179-1/1eA at −20 °C.

    Pipe ring stiffness after cooling is measured per ISO 9969:2016 with a constant loading rate of 5 mm/min; a decrease in density from 0.955 g/cm³ to 0.940 g/cm³ lowers ring stiffness by approximately 10–15%. Because RPEHD reclaim lots may contain oxidized gel, melt pressure before the screen changer is monitored continuously; a 6 MPa rise across a 200 µm screen indicates gel accumulation and triggers a screen change before melt fracture. Creep ratio is assessed by ISO 9967:2016; projected long-term modulus below 350 MPa at 50 years requires structured-wall soil support and granular embedment rather than direct burial.

    Primarily, injection molding of HDPE distribution crates and pallets is executed on 800–1,200 t toggle clamping units with multicavity stack molds and accumulator-assisted hot runner systems. Ravago HDPE RPEHD at a melt flow rate of 5–10 g/10 min per ISO 1133-1:2022 is injected at specific pressures of 80–120 MPa; holding pressure is held at 50–70 MPa for 6–10 s until gate freeze. Mold surface temperature is controlled at 18–35 °C using turbulent-flow water circulation. The semicrystalline HDPE skin freezes rapidly and releases from the core with differential shrinkage of 1.5–2.5% per ISO 294-4:2018; ejection before the part reaches dimensional stability produces diagonal warpage and corner lift.

    Lot-to-lot variability in post-consumer HDPE flake creates injection pressure curve shifts of ±8 MPa at fixed stroke. The correction is made by adjusting metering stroke rather than raising barrel temperature above 230 °C; excessive barrel temperature accelerates oxidative chain scission and lowers notched impact after 3 regrind cycles. Crate weight is held within ±1.5% of nominal; short shots are often caused by pellet bulk density variation or by blockage of 250 µm melt filtration screens. Molded crate impact resistance is verified by ASTM D2463-15 at 0 °C; loaded pallet performance is assessed under ISTA 7E. HDPE crates are not processed above 110 °C in hot wash or steam sterilization unless the part has been annealed, because permanent part distortion exceeds field tolerances.

    Geomembrane Sheet Lines, Roll Hardness, and OIT Control

    Because geomembrane sheet requires a 1.5–2.5 mm core gauge, low gel count over a 2.0–2.5 m lay-flat width, and controlled roll hardness, flat-die extrusion of Ravago HDPE RPEHD is normally performed on a 150 mm barrier screw extruder with 30:1 L/D and a coat-hanger die equipped with restrictor-bar adjustment. Melt temperature is held at 210–230 °C; the die lip gap is set 10–20% above the target sheet gauge to compensate for neck-in and draw-down. Three-roll cooling stack temperatures are staged from 45 °C to 70 °C; higher roll temperatures reduce residual stress but increase blocking tendency in roll stock.

    Oxidative induction time per ISO 11357-6:2018 at 200 °C in oxygen should exceed 100 min for geomembrane grades; stress crack resistance by ASTM D5397-20 single-point notched constant tensile load should not fail before 400 h. Carbon black dispersion is checked by ISO 18553:2018; agglomerates larger than 20 µm are defects that cause local stress concentration at weld seams. If the RPEHD feedstock contains mixed-color recyclate, carbon black masterbatch addition at 2.0–3.0 wt% is required to reach a minimum carbon black content of 2.0% per ASTM D1603-14. Published data for highly variable post-consumer RPEHD lots in geomembrane wedge weld fusion after thermal cycling is limited; prequalification trial welds are required for each incoming lot.

    When HDPE Closure Compounds Replace Polypropylene in Short-Bore Cap Molding

    Short-bore multicavity cap molds with 48 to 96 cavities operate at injection speeds of 180–250 mm/s and require a melt flow rate of 3–8 g/10 min for HDPE closure compounds. Ravago HDPE RPEHD is processed at 190–215 °C; the lower processing temperature relative to polypropylene reduces thermal degradation but increases gate frost time by 10–15% unless the hinge web is thinned. Tamper-band elongation is measured per ASTM D638-14 on molded plaques; the hinge must survive 300–500 flexural cycles without visible whitening.

    Environmental stress-crack resistance is the controlling long-term property for detergent and agrochemical caps. Testing per ASTM D1693-15 Type B should exceed 50 h at 10% Igepal; stress cracking at the tamper-band notch occurs when recycled content introduces low-molecular-weight tail fractions. In closures requiring UN certification for dangerous goods, recycled HDPE content is frequently limited to 25–35 wt% to preserve slit-tear resistance and cap engagement torque. HDPE closures are not used alone for oxygen-sensitive beverages because polyethylene oxygen permeability is typically 2,000–4,000 cm³·mm/(m²·day·atm) at 23 °C and 0% RH; a barrier liner or multi-layer structure is required.

    Melt Filtration and Surface Quality Are Controlled Separately in HDPE Conduit Lines

    Corrugated HDPE conduit produced from Ravago HDPE RPEHD is extruded on vacuum corrugators with an internal rib structure that must withstand 1,250 N crush force per ASTM D2412-21. Outer wall gauge is maintained between 1.2 mm and 1.8 mm; thinning below 1.0 mm at the corrugation crest reduces crush resistance below code requirements and creates kinking during field bending radius tests. UV resistance is provided by carbon black at 2.0–2.5 wt% with dispersion ratings better than 6 per ISO 18553:2018; without stabilization, outdoor exposure for 12–24 months causes surface embrittlement and loss of impact strength.

    Installation lubricity is influenced by the coefficient of friction between the conduit wall and cable jacket. Organosiloxane process aids are added at 0.5–1.0 wt% to reduce the dynamic coefficient of friction to 0.15–0.25 as measured by ASTM D1894-14 against steel. When post-consumer reclaim contains paper labels or adhesive residues, melt filtration at 150–200 µm is required to prevent die buildup; finer filtration raises melt pressure by 4–6 MPa over an 8 h run. Crush and impact testing follows UL 651A; joint pull-out resistance after temperature cycling from −30 °C to 60 °C must show less than 3% diametric change.

    Free Quote

    Competitive Ravago HDPE RPEHD prices that fit your budget—flexible terms and customized quotes for every order.

    For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.

    We will respond to you as soon as possible.

    Tel: +8618005193850

    Email: sales8@ascent-chem.com

    Inquiry

    Get Free Quote of Ascent Petrochem Holdings Co., Limited

    Flexible payment, competitive price, premium service - Inquire now!

    Certification & Compliance
    More Introduction

    Ravago HDPE RPEHD within the Polyethylene Density Classification

    Ravago HDPE RPEHD is a pelletised high-density polyethylene resin designated for injection moulding, extrusion blow moulding, sheet extrusion, and selected compression moulding operations. The material belongs to the high-density polyethylene class as defined by ISO 1183-1, with a density range of 0.945 g/cm³ to 0.965 g/cm³ at 23 °C. The designation RPEHD indicates a high-density polyethylene base resin distributed by Ravago; the exact melt flow rate, molecular weight distribution, additive package, and lot-specific mechanical values are recorded on the certificate of analysis. The linear HDPE backbone yields a crystalline fraction of 60 % to 80 % when determined by differential scanning calorimetry under ISO 11357-3. This crystallinity is the structural basis for the material’s flexural modulus, chemical resistance, and dimensional stability in rigid packaging. Unlike low-density polyethylene produced by high-pressure free-radical polymerisation, RPEHD has a lower degree of long-chain branching, which narrows the melting interval and accelerates solidification in cooled moulds.

    The product is not a single-viscosity commodity; it is supplied across a controlled melt flow range to suit different conversion processes. Blow moulding grades in this class typically fall between 0.2 g/10 min and 1.2 g/10 min at 190 °C/2.16 kg under ISO 1133-1. Injection moulding grades are more fluid, commonly 4.0 g/10 min to 8.0 g/10 min. The specific grade should be selected by melt flow rate rather than by density alone because cycle time and drop-impact performance move in opposite directions as melt flow rate increases. Published data for this specific RPEHD configuration is limited; therefore, design qualification must use the lot certificate rather than generic published curves.

    Incoming resin is received in 25 kg multi-wall bags, octabin bulk containers, or silo truck. Polyethylene is not hygroscopic; moisture absorption is predominantly surface condensation after storage in unheated warehouses. Where ambient relative humidity exceeds 60 % or bag surfaces show visible dew, a desiccant or tray dryer set to 60 °C to 70 °C for 1 h to 2 h removes surface moisture and prevents splay in injection-moulded parts or sheet. Prolonged drying above 80 °C is unnecessary and may accelerate oxidative degradation of the pellet surface. The feed throat should be maintained below 50 °C to prevent irregular pellet flow and bridging. Regrind addition is acceptable up to 20 % by weight in non-food applications where the regrind is produced from unpigmented, uncontaminated runner and reject parts; higher additions increase black-speck formation and melt flow shift. For food-contact articles, rework use must comply with the specific migration limits of the applicable legislation and cannot be assumed from virgin resin clearance.

    What Physical Property Envelope Is Used for Design Calculations?

    Mechanical design for load-bearing HDPE parts uses tensile yield stress and flexural modulus rather than ultimate tensile strength, because creep and stress relaxation dominate long-term performance. The following table reports the typical property envelope for the general-purpose high-density polyethylene class represented by Ravago HDPE RPEHD. Test results are generated on conditioned specimens at 23 °C and 50 % relative humidity under ISO 291 unless otherwise indicated.

    PropertyTest methodTypical range
    DensityISO 1183-10.945–0.965 g/cm³
    Melt mass-flow rateISO 1133-1, 190 °C/2.16 kg0.2–8.0 g/10 min
    Tensile yield stressISO 527-2, 50 mm/min20–30 MPa
    Flexural modulusISO 178800–1500 MPa
    Charpy notched impact at 23 °CISO 179-1/1eA4–12 kJ/m²
    Vicat softening temperatureISO 306, 50 °C/h, 50 N120–130 °C
    Heat deflection temperatureISO 75-2/B, 1.8 MPa45–60 °C
    Melting peak temperatureISO 11357-3130–137 °C
    Shore D hardnessISO 86860–70

    Environmental stress-cracking resistance is not captured by any single short-term mechanical test. For medium-molecular-weight HDPE, the F50 value under ASTM D1693 condition B, 100 % Igepal CO-630, commonly exceeds 100 h. High-flow injection grades may show F50 below 50 h because reduced tie-chain density weakens plateau resistance. The actual RPEHD lot value must be confirmed when the part contacts detergents, alcohols, or surfactant-containing agricultural chemicals. In such applications, a design stress below 4 MPa is generally required for long-term service.

    Routine lot acceptance is based on melt flow rate and density rather than full mechanical tests. Typical control tolerances for HDPE are ±0.2 g/10 min for MFR below 1.0 g/10 min, ±0.5 g/10 min for MFR above 1.0 g/10 min, and ±0.001 g/cm³ for density. A shift of 0.2 g/10 min can alter fill time by 0.5 s to 1.0 s in a multi-cavity closure tool running a 6 s cycle. Therefore, process capability studies should track melt flow rate as a primary incoming variable.

    Rheological characterisation at 190 °C using a capillary rheometer with a 30 mm length and 1 mm diameter die indicates pseudoplastic flow. The apparent viscosity at 100 s⁻¹ is commonly 1000 Pa·s to 2500 Pa·s; at 1000 s⁻¹ the viscosity falls to 200 Pa·s to 500 Pa·s. The power-law index n is typically 0.35 to 0.55, meaning that increasing shear rate reduces viscosity significantly. Melt flow rate ratio, calculated as MFR at 190 °C/21.6 kg divided by MFR at 190 °C/2.16 kg under ISO 1133-1, is a practical indicator of molecular weight distribution. For unimodal HDPE this ratio is usually 20 to 30; for bimodal pipe-grade HDPE the ratio is typically above 30. A single-point MFR is insufficient for injection moulding tool design, because two lots with the same 2.16 kg MFR can differ in high-shear fluidity and thus fill thin-wall sections differently.

    Extrudate swell during parison formation is a direct consequence of this shear-thinning and molecular relaxation behaviour. A die swell of 30 % to 50 % is typical for blow moulding grades at shear rates from 100 s⁻¹ to 400 s⁻¹. In injection moulding, gate design should limit shear rate below 100,000 s⁻¹ to avoid melt fracture and molecular scission. For a gate land length of 0.5 mm to 1.0 mm, the corresponding gate diameter is usually 0.6 mm to 1.5 mm, depending on flow length and wall stock.

    When High-Density Polyethylene Replaces LDPE, LLDPE, or Polypropylene in Rigid Applications

    Substitution of RPEHD for LDPE, LLDPE, or PP requires recalculation of shrinkage allowance, notched impact reserve, and heat resistance. HDPE has higher crystallinity than LDPE and LLDPE, which increases modulus and chemical resistance while reducing low-temperature ductility. The comparative data below use the standard test methods indicated and represent the commodity polyolefin classes, not a single production lot.

    PropertyHDPE RPEHD classLDPELLDPEPP
    Density0.945–0.965 g/cm³0.915–0.935 g/cm³0.915–0.940 g/cm³0.900–0.910 g/cm³
    Tensile yield stress20–30 MPa8–12 MPa12–20 MPa25–35 MPa
    Flexural modulus800–1500 MPa200–400 MPa300–600 MPa1000–1700 MPa
    Vicat softening120–130 °C80–95 °C90–110 °C150–160 °C
    Mould shrinkage, flow direction1.5–3.0 %1.5–3.0 %1.5–3.0 %1.0–2.0 %

    HDPE RPEHD demonstrates a sharper melting peak than LLDPE, allowing faster set-up in cooled moulds but increasing sensitivity to frozen-in orientation. When replacing PP, the lower Vicat softening temperature of HDPE limits hot-fill packaging above 80 °C, whereas PP retains stiffness to higher temperatures. In aggressive detergent environments, HDPE often outperforms PP in ESCR, provided the moulded-in stress is below the threshold noted earlier. The transition from PP to HDPE on an injection moulding machine also requires a residence-time adjustment: because HDPE has higher specific heat and different thermal conductivity, screw recovery and barrel temperature profiles should be verified with short-shot studies before production changeover.

    Compared with a bimodal PE 100 pipe-grade HDPE, the RPEHD class is lower in ESCR plateau and not optimised for hydrostatic pressure rating. Pipe-grade HDPE may have an MFR below 0.3 g/10 min and a melt flow ratio above 30; such values are unsuitable for thin-wall injection moulding because filling pressure becomes excessive. Conversely, high-flow HDPE injection grades with MFR above 20 g/10 min are unsuitable for large parison blow moulding because their low melt strength produces parison drawdown.

    Mould shrinkage for unfilled HDPE is anisotropic and time-dependent. Under ISO 294-4, mould shrinkage measured after 24 h at 23 °C and 50 % relative humidity is typically 1.5 % to 2.5 % in the flow direction and 1.0 % to 2.0 % transverse to flow. After 48 h additional crystallinity development may add 0.1 % to 0.3 % shrinkage. Wall thickness variations from 1.5 mm to 3.0 mm can create differential shrinkage of 0.4 % to 0.8 %, producing warpage in rectangular containers. Tooling dimensions for critical fits should be verified with prototype shots at the intended production melt temperature and mould temperature, not from datasheet values alone. In extrusion blow moulding, parison sag and swell interact with mould pinch-off geometry; a blow ratio above 3:1 increases wall-thinning and reduces top-load capacity unless the parison is programmed with a diverging die gap.

    ESCR, Moisture Ingress, and Additive Compatibility Boundaries

    The environmental stress-cracking resistance of HDPE RPEHD depends on comonomer type, molecular weight, and processing history. The test method ASTM D1693 condition B uses 100 % Igepal CO-630 at 50 °C; F50 values vary from below 50 h for low-viscosity injection grades to above 300 h for high-molecular-weight blow moulding grades. A moulded-in stress above 4 MPa in contact with detergent solutions can reduce service life even when the laboratory ESCR value is acceptable. The material is not recommended for continuous contact with strong oxidising acids above 60 °C or aliphatic solvents above 40 °C. Swelling in hexane and similar solvents can reduce tensile yield stress by more than 10 % in 24 h. Amine-based additives and certain solvent-borne colour concentrates should be avoided at processing temperatures above 240 °C, because interactions with residual catalyst acidity may generate odorous by-products. Calcium stearate or zinc stearate external lubricants are acceptable at loadings up to 0.1 % by weight; above that level, plate-out on mould surfaces and interference with surface adhesion become detectable.

    On a 25:1 L/D single-screw extruder with a barrier screw and Maddock mixing section, a typical HDPE RPEHD barrel profile runs from 180 °C at the feed zone to 220 °C at the metering zone. Extrusion blow moulding lines with grooved feed throats operate at die-head temperatures of 200 °C to 230 °C. A clamp force of 1.5 kN/mm² of projected area is a conservative starting point for injection moulding. Melt temperature should be set from 190 °C to 240 °C, with mould surface temperature from 15 °C to 50 °C. If mould temperature falls below 15 °C, the replication of fine texturing is incomplete and surface gloss may drop below 60 % under ASTM D2457. Back pressure of 0.5 MPa to 1.5 MPa maintains melt homogeneity without excessive screw recovery delay. Shear rates above 100,000 s⁻¹ in gates and runners produce melt fracture and possible odour. For sheet extrusion, a die gap of 0.8 mm to 2.0 mm and chill-roll temperature of 40 °C to 60 °C produce haze below 15 % and gloss above 60 %. Process deviations observed on production-scale lines include parison sag exceeding 15 % of initial length when melt temperature exceeds 220 °C, and screw recovery time increasing by 10 % to 20 % when back pressure is raised above 1.5 MPa.

    Regulatory Status under FDA 21 CFR 177.1520 and EU 10/2011

    In the United States, high-density polyethylene homopolymer is covered by FDA 21 CFR 177.1520 for food-contact articles, subject to density, melt index, and extraction limits. Compliance is not automatic for colour masterbatches, processing aids, or reclaimed resin, which must be evaluated separately. In the European Union, plastics intended for food contact are regulated by Commission Regulation (EU) No 10/2011; the overall migration limit is 10 mg/dm² or 60 mg/kg for food simulants specified by the regulation. HDPE food-contact articles are typically tested in simulant D1 or D2 with time-temperature conditions appropriate to the intended use. REACH compliance requires that no substance of very high concern be present above 0.1 % by weight. RoHS Directive 2011/65/EU restricts lead, mercury, cadmium, hexavalent chromium, polybrominated biphenyls, and certain polybrominated diphenyl ethers; the base HDPE generally meets these limits, but component-level verification is required after pigmentation and additive incorporation.

    Blow-moulded containers for liquid detergents, oils, and agricultural chemicals are produced with a die swell of 30 % to 50 % and a blow ratio of 2:1 to 4:1. The parison melt temperature is held between 190 °C and 220 °C; below this range sharkskin melt fracture appears on the parison surface, and above this range parison sag exceeds 15 % of initial length. Injection-moulded caps and closures use valve-gated hot-runner tools with gate diameters of 0.8 mm to 1.2 mm; pack pressure of 70 MPa for 1.5 s to 3.0 s prevents sink marks. Crates and pallets with wall thickness above 4 mm require cooling times estimated from the square of wall thickness; for a 4 mm wall at 20 °C mould temperature, cooling time is approximately 15 s to 20 s. Small-diameter conduit extrusion is possible but is not the primary design envelope for this grade; screw speed should be limited to 60 rpm on a 30:1 L/D extruder to limit molecular scission. For sheet used in thermoformed trays, the extruded sheet should be wound at a surface temperature below 40 °C to prevent blocking in roll form.

    Top