| HS Code | 379337 |
| Density | 0.954 g/cm³ |
| Melt Flow Rate 190 C 21 6 Kg | 4.0 g/10 min |
| Tensile Strength At Yield | 28 MPa |
| Tensile Elongation At Break | >600% |
| Flexural Modulus | 1200 MPa |
| Vicat Softening Point | 126 °C |
| Melting Point | 131 °C |
| Environmental Stress Crack Resistance F50 100 Igepal | >1000 h |
| Shore D Hardness | 65 |
| Charpy Notched Impact Strength 23 C | 15 kJ/m² |
| Thermal Conductivity | 0.4 W/mK |
| Coefficient Of Linear Thermal Expansion | 1.3 x 10^-4 /°C |
| Water Absorption | <0.01% |
| Dielectric Constant 1 Mhz | 2.3 |
| Volume Resistivity | >10^15 ohm-cm |
As an accredited QAPCO HDPE LOTRÈNE TR-144 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | QAPCO HDPE LOTRÈNE TR-144 is supplied in 25 kg polyethylene bags, palletized for industrial handling and transport. |
| Container Loading (20′ FCL) | 20′ FCL container loaded with QAPCO HDPE LOTRÈNE TR-144 in 25 kg bags, palletized, shrink-wrapped, and secured for ocean shipment. |
| Shipping | QAPCO HDPE LOTRÈNE TR-144 is shipped as a non-hazardous thermoplastic, typically in 25 kg polyethylene bags, palletized and stretch-wrapped. It is transported in clean, dry containers or covered trucks, protected from moisture, direct sunlight, and excessive heat. No UN hazard class or special placarding required. Handle carefully to avoid bag damage. |
| Storage | Store QAPCO HDPE LOTRÈNE TR-144 in a cool, dry, well-ventilated warehouse, away from direct sunlight, heat, flames, and oxidizers. Keep original bags or containers tightly closed and off the floor on pallets. Avoid moisture, dust, and physical damage. Stack securely to prevent collapse. Use suitable PPE during handling. Maintain good housekeeping and follow local storage regulations. Ensure adequate ventilation. |
| Shelf Life | QAPCO HDPE LOTRÈNE TR-144 shelf life is typically 12 months in original, unopened packaging, stored cool, dry, away from sunlight. |
In jurisdictions where single-use retail carry-out sacks remain lawful under local legislation, QAPCO HDPE LOTRÈNE TR-144 is processed on high-stalk blown film lines with grooved-feed extruders of 30:1 to 40:1 L/D ratio, barrier screws, and die diameters from 600 mm to 2,000 mm. The resin’s nominal density of 0.944 g/cm³ per ISO 1183-1:2019 and MFR of 0.18 g/10 min at 190°C/2.16 kg per ISO 1133-1:2022 place it in the high-molecular-weight film class. A typical formulation for high-speed conversion comprises 90–100 wt% TR-144 and 0–10 wt% LLDPE-butene grade to stabilize bubble geometry; the LLDPE fraction is not added as a lubricant but as a melt-fracture suppressant. Process conditions on production lines include melt temperature 193–210°C, die gap 1.6–2.4 mm, blow-up ratio 3.0:1–4.0:1, and neck height 8–12 die diameters. At these settings, frost-line instability is observed below 8 die diameters, causing gauge variation exceeding ±8% in high-speed post-neck collapsing. Compliance is verified against ISO 7765-1:1988 dart impact and ISO 6383-2:2003 Elmendorf tear, with converted rollstock subjected to a minimum dart drop of 300 g F50 at 10 µm film thickness on typical production samples. Terminal product types include die-cut T-shirt sacks, wicket blocks for retail produce, and perforated roll bags for bakery dispense boxes; all require low gel counts because fish-eye defects initiate impact failure at perforation points during high-speed conversion.
Industrial refuse sacks and heavy-gauge drum liners produced from TR-144 are specified under EN 13592:2012 for household waste collection sacks, with dimensional stability, tear resistance, and impact resistance measured by methods referenced in that standard. Formulation shift to 70–90 wt% TR-144, 10–30 wt% clean post-consumer HDPE regrind, and 2–3 wt% carbon black masterbatch is production-validated on grooved-feed blown film lines with screen changers operating at 3–5 MPa head pressure. The regrind fraction introduces batch-to-batch variability in melt viscosity; when recycled content exceeds 30 wt%, the melt index shifts upward relative to virgin TR-144, and dart impact measured under ISO 7765-1:1988 drops by more than 25% at 50 µm gauge in production trials. Extruder zones are set at 180°C feed, 200°C compression, 210°C metering, and die temperature 205°C, with die gap held at 2.0 mm to prevent sharkskin at high output. Terminal products include 60–120 L bin liners, contractor bags, laundry bags, and drum liners for non-hazardous solids; medical waste sacks require separate validation against healthcare packaging regulations and are outside this classification without documented incinerability and sterilization compatibility testing.
Monolayer food-contact blown film for cereal carton liners, biscuit wraps, and dry pouches is produced with TR-144 at 100 wt% virgin resin, except where a 5–10 wt% neat LDPE companion resin is added to improve transverse direction tear at 20–40 µm gauge. Compliance rests on FDA 21 CFR 177.1520 for olefin polymers and EU 10/2011, with overall migration testing according to EN 1186-1:2002 and specific migration limits for chromium, cadmium, lead, and mercury as specified in EU 10/2011 Annex II. Production is fixed on barrier-screw blown film equipment with polished die lips and no recycled content; process water and air handling must limit dust, as gel defects above 0.3 mm create leak paths at heat-seal corners. Extrusion melt temperature is maintained at 185–205°C to avoid oxidative by-products that impart off-taste; line-specific sensory panels evaluate off-odor on filled packages after 24 h at 40°C. The film is converted into pre-made pouches, form-fill-seal rollstock for dry breakfast cereals, and glassine-replacing bag-in-box liners. In food-contact service, operators must not substitute PCR or post-industrial scrap unless the substitution is cleared under a food-contact suitability opinion from the competent authority.
Three-layer blown-film coextrusion for e-commerce mailer films and lightweight packaging uses TR-144 in the core at 30–50 wt%, LLDPE-butene or LLDPE-octene seal layers at 20–35 wt%, and recycled HDPE middle layer at 20–40 wt%, depending on virgin material availability. Packaging compliance is verified against 94/62/EC heavy-metal limits and, for US shipments, CONEG Model Legislation concentrations of lead, mercury, cadmium, and hexavalent chromium below 100 ppm total. The core layer’s high melt strength stabilizes the bubble when total film gauge is reduced from 60 µm to 45 µm on a 1,600 mm die; the die gap is opened from 1.8 mm to 2.2 mm relative to monolayer processing to maintain the same die pressure and avoid melt fracture. Layer distribution is controlled by gravimetric feeders, and cross-web thickness variance is held within ±5% using an internal bubble cooling system with segmented air rings. Terminal products include opaque poly mailers, padded mailer outer films, and void-fill overwrap; if the structure is used as a mailer, seal strength is tested per ASTM F88/F88M-21 at 2.5 N/25 mm minimum after 24 h conditioning at 23°C/50% RH. The downgauging limit is constrained by dart impact; below 45 µm total gauge, field returns increase along fold edges unless the LLDPE skin layer fraction is raised above 35 wt%.
Construction membrane extrusion from TR-144 targets under-slab vapour retarders with thickness from 0.15 mm to 0.25 mm, laid-flat widths up to 6 m, and low-temperature impact resistance verified under ASTM E1745-17. The compound consists of 96–97 wt% TR-144 and 3–4 wt% carbon black masterbatch, with no post-consumer regrind in the primary membrane layer; if a three-layer coextrusion line is used, the inner core may contain 15–20 wt% plant scrap. Extrusion uses a 105 mm grooved-feed extruder with 33:1 L/D, melt temperature 204–218°C, die gap 2.4–2.8 mm, and blow-up ratio 2.8:1–3.5:1; output rates on wide-width lines reach 350–450 kg/h without exceeding melt pressure beyond 45 MPa. Terminal products include under-slab vapour barriers, crawl-space liners, temporary wall sheathing, and concrete curing covers. The membrane is not specified for potable water contact unless independent NSF/ANSI 61 certification is secured. Published field data for TR-144 in this exact configuration is limited, but extruder trials show that carbon black dispersion below 20 µm mean particle size is required to avoid pinholes at 0.15 mm gauge; filtration through 250 µm screen packs is standard.
Agricultural silage clamp covers and temporary fumigation sheets are extrusion-processed from a blend of 70–85 wt% TR-144, 10–25 wt% LLDPE-octene, and 5 wt% carbon black/UV stabilizer masterbatch; the LLDPE fraction maintains low-temperature flexibility at 4°C during late-season pulling. Industry compliance is evaluated under EN 13206:2017 for thermoplastic covering films for agricultural and horticultural use, with mechanical testing referencing ISO 527-3:2018 tensile properties, ISO 6383-2:2003 tear resistance, and ISO 7765-1:1988 impact resistance. Production on blown film lines with layflat width up to 12 m uses a die gap of 2.2–2.6 mm, melt temperature 200–215°C, and blow-up ratio 2.2:1–3.0:1; stationary scaffolds remove web folds before winding. Terminal products include silage clamp covers, temporary fumigation sheets, and grain bunker covers. Long-term greenhouse glazing is not specified for TR-144 unless a separate multi-year UV stability test under ISO 4892-2:2021 demonstrates more than 12,000 h retained elongation; published data for this specific TR-144 configuration is limited.
| Application scenario | Regulatory/technical framework | Test method / code | Typical limit or condition |
|---|---|---|---|
| Retail carry-out sacks | Impact and tear performance | ISO 7765-1:1988, ISO 6383-2:2003 | F50 dart drop minimum 300 g at 10 µm |
| Industrial refuse sacks | Household waste collection sacks | EN 13592:2012 | PCR fraction not to exceed 30 wt% without revalidation |
| Food-contact liners | Olefin food-contact compliance | FDA 21 CFR 177.1520, EU 10/2011, EN 1186-1:2002 | Overall migration per EU 10/2011 Annex II |
| E-commerce mailers | Heavy-metal packaging limits | 94/62/EC, CONEG Model Legislation | Heavy metals < 100 ppm total |
| Under-slab vapour retarders | Flexible water vapour retarders | ASTM E1745-17 | Thickness 0.15–0.25 mm, potable water requires NSF/ANSI 61 |
| Agricultural covers | Thermoplastic covering films | EN 13206:2017, ISO 4892-2:2021 | Long-term glazing only with confirmed UV stability |
| Application scenario | TR-144 addition ratio | Co-resins / additives | Process thickness range |
|---|---|---|---|
| Retail carry-out sacks | 90–100 wt% | 0–10 wt% LLDPE-butene | 8–20 µm |
| Industrial refuse sacks | 70–90 wt% | 10–30 wt% PCR-HDPE, 2–3 wt% carbon black | 30–70 µm |
| Food-contact liners | 100 wt% virgin | 0–10 wt% LDPE | 20–40 µm |
| E-commerce mailers | 30–50 wt% | 20–35 wt% LLDPE, 20–40 wt% recycled HDPE | 45–60 µm |
| Under-slab vapour retarders | 96–97 wt% | 3–4 wt% carbon black masterbatch | 0.15–0.25 mm |
| Agricultural covers | 70–85 wt% | 10–25 wt% LLDPE-octene, 5 wt% UV/black masterbatch | 0.10–0.20 mm |
Competitive QAPCO HDPE LOTRÈNE TR-144 prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
QAPCO HDPE LOTRÈNE TR-144 is a high-density polyethylene produced by Qatar Petrochemical Company under the Lotrene brand and classified in the technical datasheet as an extrusion blow moulding resin. Published typical values include a melt flow rate of 0.30 g/10 min when determined according to ISO 1133-1 at 190 °C under 2.16 kg and a density of 0.946 g/cm³ measured by ISO 1183-1. The combination places TR-144 in the low-flow, medium-high-density segment of HDPE, where high melt tenacity is required for parison stability and moderate crystallinity is required for stacking strength and environmental stress crack resistance. The grade is not intended for thin-film extrusion, injection moulding, or rotomoulding because the high viscosity at low shear would produce excessive motor loads, poor melt distribution, and incomplete cavity filling in those processes.
The melt flow rate of 0.30 g/10 min is a low-shear index and does not fully describe behaviour in a blow moulding die. At the higher shear rates encountered in parison extrusion, the resin exhibits shear thinning, but the public datasheet does not provide capillary rheometry curves; lot-specific oscillatory or capillary data should be obtained for tooling design. The resin is supplied as pellets, and the grade is specified by QAPCO for large industrial containers, jerrycans, and technical blow moulded parts.
The primary differentiator is melt flow rate. Blow moulding grades such as TR-144 are specified below 0.5 g/10 min because low viscosity would allow the molten tube to stretch under its own weight before the mould closes. Film-grade HDPE resins are typically supplied at 0.7 g/10 min to 2.0 g/10 min to allow thin melt films to be drawn across a die lip at high throughput. Injection-moulding HDPE grades are higher-flow, commonly 4 g/10 min to 20 g/10 min, to fill complex tool geometries and minimize injection pressure. The 0.946 g/cm³ density of TR-144 is lower than that of highly crystalline injection HDPE at 0.952 g/cm³ to 0.962 g/cm³, which reduces crystallinity and improves environmental stress crack resistance while moderately lowering flexural modulus.
Compared with butene-LLDPE grades of similar melt index, TR-144 has a higher density and greater tensile yield stress. Butene-LLDPE cast-film grades typically exhibit tensile yield values of 10 MPa to 18 MPa under ISO 527-2, whereas TR-144 is published at 26 MPa. The difference arises from short-chain branching and crystal density; LLDPE retains a higher concentration of short-chain branches that interrupt lamellar packing. The trade-off is puncture and tear resistance, which are lower in HDPE than in LLDPE under equivalent section thickness.
Against low-density polyethylene, TR-144 has a density advantage of approximately 0.02 g/cm³ to 0.03 g/cm³ and a correspondingly higher tensile yield stress, but it lacks the high melt elasticity of high-pressure LDPE used in collapse-resistant squeeze tubes. The selection of TR-144 is therefore specific to rigid blow moulded packaging rather than flexible or squeezable articles.
On continuous shuttle blow moulding machines fitted with 65 mm single-screw extruders and 25:1 L/D barrels, TR-144 is processed at melt temperatures of 180 °C to 210 °C and die temperatures of 190 °C to 210 °C. Barrel profiles are typically set from 160 °C at the feed throat to 200 °C at the metering section, with a screen pack of 20/40/60 mesh to generate backpressure and remove contamination. A barrier screw with a compression ratio of 2.5:1 to 3.0:1 and a Maddock mixing head disperses colour and regrind without excessive shear heating. Die swell for this grade is sensitive to die land length and shear rate; short land lengths increase parison diameter and can complicate container weight distribution. Parison programming is required for non-round parts, with wall thickness profiles adjusted to increase mass at pinch-off and handle zones.
The low melt flow rate limits cycle speed in small containers. On multi-cavity machines, melt fracture and shark skin appear below 175 °C if die exit velocity is too high. Conversely, melt temperatures above 215 °C produce odour, gel formation, and loss of melt strength. Moisture absorption is negligible, but condensation on pellets stored in high-humidity environments should be removed by drying at 75 °C for 2 h because surface moisture can create splay and pinhole defects in the parison.
On accumulator-head machines used for 20 L containers, parison sagging is controlled by the melt flow rate, but large-diameter tools require extruder head pressures of 120 bar to 180 bar; excessive pressure increases shear heating and can raise the melt temperature above the recommended limit. The use of a spiral mandrel die is not necessary, but a diverging die body reduces localized high shear and die lines. Blow pins and neck rings should be maintained at 10 °C to 30 °C. Pinch-off inserts with a sharp land angle of 15° to 30° and a flash pocket depth of 0.3 mm to 0.5 mm improve weld-line strength. The parison programmer stroke should be tuned so that the thickest wall section is placed at the container shoulder and handle bridge, where top-load failure initiates.
The table below consolidates published typical values for TR-144. These values are not batch specification limits; they are laboratory characterizations on compression-moulded or injection-moulded specimens depending on the test standard. Batch-specific COA values should be requested for lot acceptance.
| Property | Typical value | Test standard |
| Melt flow rate | 0.30 g/10 min | ISO 1133-1, 190 °C, 2.16 kg |
| Density | 0.946 g/cm³ | ISO 1183-1 |
| Tensile yield strength | 26 MPa | ISO 527-2, 50 mm/min |
| Elongation at break | >600% | ISO 527-2 |
| Flexural modulus | 1100 MPa | ISO 178, 2 mm/min |
| Shore D hardness | 62 | ISO 868 |
| Vicat softening temperature | 125 °C | ISO 306/A50, 10 N, 50 °C/h |
| Brittleness temperature | <-75 °C | ASTM D746 |
| Environmental stress crack resistance | >40 h F50 | ASTM D1693, condition B, 100% Igepal |
Melt flow rate to ISO 1133-1 and density to ISO 1183-1 are the two most common lot acceptance criteria. Tensile properties are measured on ISO 527-2 type 1A specimens at 23 °C and 50 mm/min; flexural modulus is measured at 2 mm/min according to ISO 178. The Vicat softening point under load uses 10 N and 50 °C/h according to ISO 306/A50. These details permit direct comparison with other HDPE blow moulding grades if the specimen preparation method and conditioning are identical.
Because the grade is used in 5 L to 25 L industrial jerrycans and agricultural chemical containers, the critical processing defects are not only dimensional but also structural. Production-scale observations on shuttle blow moulding lines include parison curl when die-lip temperatures vary by more than 5 °C across the circumference, weld-line cracking at the pinch-off when the mould closing speed is too low, and brittle failure at the handle root when the wall thickness drops below 0.8 mm. Pinch weld strength is improved by maintaining a weld-line temperature above 180 °C and closing the mould before the parison cools below the crystalline solidification point. Top-load testing of finished containers generally follows ISO 12048 or the customer’s specific compression fixture.
Drop impact is evaluated using filled containers conditioned at -18 °C for 24 h; the failure mode in TR-144 is typically ductile hinge fracture before a weld-line split if the wall distribution is optimized. Published data for lot-specific drop-impact values in TR-144 are limited because the value depends strongly on part design, mould temperature, and closure system. Container qualification therefore requires pilot trials on the production tool. For dangerous goods packaging, containers must pass leakproofness, hydrostatic pressure, drop, and stack tests under the applicable ADR 6.1.5 provisions; passing these tests is a function of moulded wall thickness, weld geometry, and closure design as well as resin selection.
For UN-type jerrycans, the drop test height for pack group II at liquid density 1.2 kg/L is 1.2 m; pack group III uses 0.8 m. The crystalline morphology of TR-144 at a wall thickness of 1.2 mm may pass at -18 °C, but published data for this specific container configuration is limited. Moulding trials are required to establish the minimum wall thickness at the pinch weld because impact energy concentrates there.
Environmental stress crack resistance in HDPE is inversely related to density and crystallinity. TR-144, at 0.946 g/cm³, is designed to maintain a higher ESCR than injection HDPE grades at 0.952 g/cm³ to 0.962 g/cm³. The difference is material, measured under ASTM D1693, condition B, where injection grades often yield F50 values below 20 h, while blow moulding grades are commonly above 40 h. The table below illustrates the directional comparison between resin classes.
| Parameter | TR-144 | HDPE film | HDPE injection | Butene LLDPE film |
| Melt flow rate | 0.30 g/10 min | 0.7–2.0 g/10 min | 4–20 g/10 min | 0.5–2.0 g/10 min |
| Density | 0.946 g/cm³ | 0.944–0.958 g/cm³ | 0.952–0.962 g/cm³ | 0.918–0.925 g/cm³ |
| Tensile yield stress | 26 MPa | 22–29 MPa | 28–32 MPa | 10–18 MPa |
| Flexural modulus | 1100 MPa | 900–1300 MPa | 1300–1700 MPa | 250–450 MPa |
| ESCR trend | High | Medium | Low to medium | High |
| Primary process | Extrusion blow moulding | Film extrusion | Injection moulding | Cast or blown film |
The comparative table is directional and should not be used as a specification. Grade-specific data for film, injection, and LLDPE resins vary by comonomer type, molecular weight distribution, and additive package. Within the QAPCO Lotrene HDPE range, TR-144 is positioned as a high-molecular-weight blow moulding grade rather than a high-flow injection or film grade. The numerical suffix should not be interpreted as a composition code without consulting the QAPCO technical datasheet. Grade selection between TR-144 and other QAPCO HDPE resins is governed by the required melt flow rate and container volume. Published data for direct comparative testing of TR-144 against other Lotrene HDPE grades in the same moulding tool is limited; end users should request QAPCO technical support and COA documentation for the alternative grades.
Against high-density polyethylene blow moulding grades with density 0.950 g/cm³ to 0.954 g/cm³, TR-144 may show lower top-load stiffness but better ESCR. Conversely, against lower-density HDPE at 0.940 g/cm³, TR-144 yields higher stiffness and lower impact. The density selection is therefore a compromise for balanced packaging performance. Environmental stress crack resistance of TR-144 is improved by avoiding excessive melt temperatures and by minimizing gate scarring on the pinch weld. The ESCR test under ASTM D1693 is sensitive to specimen thickness, stress concentration, and Igepal concentration; values obtained on compression-moulded sheets may not predict the performance of a moulded handle root or weld line.
Clean in-house regrind of TR-144 from post-industrial containers is generally used at 10 wt% to 20 wt%; higher levels reduce melt strength and ESCR and require revalidation of pinch weld integrity. The grade should not be blended with high-flow HDPE injection regrind without adjusting the melt flow ratio, because viscosity mismatch can produce streaks and uneven parison thickness. Colour masterbatches should be HDPE-based and should not exceed 3 wt% unless the carrier resin is matched to the melt flow range of the base polymer. Storage should avoid direct sunlight and temperatures above 50 °C to limit oxidative induction time drift. Compliance with food contact regulations, including FDA 21 CFR 177.1520 and EU 10/2011, must be verified for the specific formulation and lot.