| HS Code | 316466 |
| Product Name | QAPCO HDPE HXM50100 |
| Manufacturer | Qatar Petrochemical Company (QAPCO) |
| Polymer Type | High Density Polyethylene (HDPE) |
| Comonomer | Hexene-1 |
| Density | 0.950 g/cm3 |
| Melt Flow Rate 190 C 2 16 Kg | 10 g/10 min |
| Tensile Strength At Yield | 25 MPa |
| Tensile Strength At Break | 20 MPa |
| Elongation At Break | >1000% |
| Flexural Modulus | 1100 MPa |
| Izod Impact Strength Notched 23 C | 50 J/m |
| Vicat Softening Point | 125°C |
| Heat Deflection Temperature 0 45 Mpa | 70°C |
| Shore D Hardness | 60 |
| Melting Point | 130°C |
| Crystallinity | 65% |
| Mold Shrinkage | 1.5-3.0% |
| Water Absorption | <0.01% |
| Thermal Conductivity | 0.4 W/m·K |
| Dielectric Constant | 2.3 |
| Volume Resistivity | >1×10^16 Ω·cm |
| Form | Pellets |
| Color | Natural |
| Specific Gravity | 0.950 |
As an accredited QAPCO HDPE HXM50100 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | QAPCO HDPE HXM50100 is packaged in 25 kg moisture-resistant bags or 1,000 kg jumbo bags, palletized for industrial shipment. |
| Container Loading (20′ FCL) | QAPCO HDPE HXM50100 high-density polyethylene, loaded in 20′ FCL: 25 kg bags, palletized; approximately 18–20 metric tons per container. |
| Shipping | QAPCO HDPE HXM50100 is shipped as a non-hazardous solid in 25 kg polyethylene bags on pallets, stretch-wrapped and labeled. Transport in clean, dry containers or trucks; protect from moisture, direct sunlight, heat, and punctures. Store in a cool, ventilated area away from ignition sources. |
| Storage | Store QAPCO HDPE HXM50100 in a dry, covered, well-ventilated warehouse at ambient temperature, away from direct sunlight, heat, flames, and strong oxidizers. Keep original bags sealed on pallets, avoiding moisture, dust, and contamination. Rotate stock FIFO; prevent high stacking and damage. Use grounding to control static during handling. Inspect packaging regularly. Protect from UV light and ignition sources. |
| Shelf Life | Recommended shelf life: typically 2 years when stored in original unopened packaging, protected from direct sunlight, heat, moisture, and contamination. |
In potable water transmission and distribution piping, QAPCO HDPE HXM50100 is applied as a ready-to-use high molecular weight PE100 pressure pipe compound whose hydrostatic design basis is established under ISO 9080:2012 and ISO 12162. The compound’s melt flow rate under 190 °C/5.0 kg load is typically 0.10 g/10 min, placing it in the high-viscosity range required for thick-wall pipe extrusion. Compliance for potable water contact is evaluated against EN 12201-1:2011 and ISO 4427-1:2019; where specified for UK or North American markets, hygienic testing follows BS 6920-1:2000 or NSF/ANSI/CAN 61:2020. The feed is 100 wt% pellet basis with carbon black content 2.0–2.5 wt% and a stabilizer package; clean in-house regrind from the same grade may be added up to 5 wt%, while dilution with higher-MFR HDPE beyond 10 wt% is not recommended because it lowers slow crack growth resistance and invalidates the PE100 design envelope. Downstream conversion on single-screw grooved-barrel extruders with L/D 30:1–36:1 uses barrel zone set points of 180–210 °C and head/die temperatures of 200–215 °C; screen pack pressure in production lines typically rises from 18 MPa to 28 MPa as gels accumulate, and the melt-pressure differential triggers screen replacement before melt fracture occurs. Vacuum calibration tanks maintain cooling water at 15–25 °C; pipes above 250 mm OD require internal air cooling or extended submerged quenching to prevent sink marks and centerline shrinkage. Finished product forms consist of blue or black-with-blue-stripe PE100 water mains and service laterals from 20 mm to 630 mm OD, fabricated in SDR 26, 17, 13.6, and 11 dimensions for nominal pressure ratings from 6.3 bar to 25 bar.
Rapid crack propagation is the controlling failure mode for PE100 gas distribution pipe, and HXM50100 is converted into gas piping only after batch verification under ISO 13477:2008 at 0 °C with the S4 critical pressure criterion. The main wall is fed at 100 wt% HXM50100 black compound; no external regrind is used in gas service. A coextruded yellow identification stripe made from a pigmented PE100 or PE80 compound typically constitutes 3–5 wt% of total wall mass, and the stripe layer must not reduce the main wall below the SDR minimum specified in ISO 4437-1:2014 or EN 1555-1:2010. North American projects may require ASTM D2513-20 and CFR 49 Part 192 marking, but material alone does not determine compliance because fusion joint quality under ISO 21307:2017 also governs system certification. Production uses grooved-feed single-screw extruders with L/D 33:1–36:1, barrel set points 190–220 °C, spiral mandrel die temperatures 210–225 °C, and vacuum sizing to maintain ovality below 1.5% of OD. Slow crack growth resistance is assessed on notched pipe per ISO 13479 at 80 °C and 4.6 MPa, with PE100 batches required to exceed 500 h before failure. The extruded pipe range includes black PE100 gas mains and service pipes from 20 mm to 400 mm OD in SDR 11 and SDR 17.6, supplied in straight lengths or coils up to 160 mm OD, with butt-fusion joints using heater plate temperatures of 220–230 °C.
Mining tailings and dredging discharge systems select HXM50100 less for its pressure rating than for its high molecular weight and thick-wall processing stability under repeated solids impingement. Pressure containment follows ISO 4427-2:2019 and, where applicable, AS/NZS 4130:2018 or ASTM F714-21; published data for slurry abrasion life of this specific configuration is limited, so field wear rates from production-scale tailings lines are the accepted design basis. The extrusion formulation is normally 100 wt% HXM50100 black compound with no filler; pipe wall thickness is specified at 1.3–1.5 times the pressure-rated minimum to provide sacrificial wear allowance. Conversion on large-bore pipe lines uses grooved-feed single or twin-stage extruder arrangements, L/D 30:1–36:1, spiral mandrel dies, and melt temperatures kept in the 190–210 °C band to avoid polymer degradation during extended campaigns. Thick walls above 50 mm require internal air cooling and stepped vacuum tanks because outer-surface-only heat removal otherwise causes sidewall voids and uneven crystallinity. Delivered pipe configurations cover tailings transport mains from 110 mm to 1000 mm OD, dredge discharge lines with flanged HDPE stub ends, and slip-lined wear pipes installed inside steel casings; butt fusion joints follow ISO 21307:2017 at heater plate temperatures of 220–230 °C.
Pressurized sewer force mains made from HXM50100 are specified where pumped wastewater, sludge, or septic tank effluent is conveyed at intermittent flow regimes that generate hydrogen sulfide and low-pH condensate on the pipe wall. Material compliance is held to AWWA C906-21 for PE pressure pipe and fittings in water and wastewater, alongside EN 12201-1:2011 and ISO 4427-1:2019 for PE100 classification; jointing is governed by ISO 21307:2017. The extrusion feed is 100 wt% HXM50100 black compound with 2.0–2.5 wt% carbon black; clean in-house regrind from the same lot is limited to ≤5 wt%, and no chlorinated additives or external filler are introduced because they reduce slow crack growth resistance and pressure derating under aerobic sludge exposure. Conversion uses grooved-feed single-screw extruders with L/D 30:1–36:1, barrel set points 180–210 °C, die head 200–215 °C, and vacuum calibration to hold wall thickness tolerances consistent with ISO 11922-1. Finished pipe classes include 63–630 mm OD PE100 sewer rising mains, sludge transfer lines, and digester feed pipes in SDR 11, 13.6, and 17, joined by butt fusion at 220–230 °C heater plate temperatures.
Corrugated drainage pipe manufactured from HXM50100 is governed by ASTM F2306/F2306M-20 and AASHTO M294:2018 for storm sewers and culverts, with pipe stiffness requirements referenced to ASTM D2412/D2412M-21 at 5% deflection. The recipe uses 100 wt% black HXM50100 pellets; because the compound already contains carbon black at 2.0–2.5 wt%, no additional UV masterbatch is required. Corrugator lines run a melt temperature of 210–225 °C through a rectangular die lip opening of 1.0–2.5 mm, after which vacuum forming onto moving mold blocks with 0.03–0.06 MPa vacuum shapes the corrugations. Product geometries span 150–1200 mm ID dual-wall and single-wall corrugated storm drains, highway underdrains, retention/detention system laterals, and perforated agricultural drainage lines.
For industrial chemical effluent and firewater mains, HXM50100 is processed as an unplasticized PE100 compound whose chemical resistance is appraised against ISO/TR 10358 and DIN 8075-1; pressure design follows ISO 4427-2:2019, and butt-fusion joint qualification is governed by ISO 21307:2017. The feed is 100 wt% HXM50100 black compound; no color masterbatch is added when black identification is acceptable, and any in-house regrind is limited to ≤5 wt% and restricted to non-potable service. Extrusion conditions overlap potable water pipe production: grooved-barrel single-screw machines with L/D 30:1–36:1, barrel temperatures 180–210 °C, and die temperatures 200–215 °C. End-use product types are chemically resistant PE100 pipes for acidic or alkaline effluent, firewater ring mains, and industrial wastewater lines in 20 mm to 630 mm OD, especially where external corrosion of steel is a reliability issue. The operational boundary is explicit: HXM50100 is not rated for aromatic hydrocarbon service or strong oxidizing media at temperatures above 40 °C, and published data for this specific configuration is limited for mixed-solvent streams, so compatibility testing is required before deployment.
Competitive QAPCO HDPE HXM50100 prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
QAPCO HDPE HXM50100 is a bimodal high-molecular-weight high-density polyethylene developed for thin-gauge blown film extrusion. The grade is specified in QAPCO technical literature by a nominal density of 0.950 g/cm³ measured according to ISO 1183-1 and a high-load melt index of 10.0 g/10 min at 190°C and 21.6 kg measured according to ASTM D1238-13 Condition F or ISO 1133-1:2022. The molecular weight distribution is broad and intentionally nonuniform; the low-molecular-weight fraction contributes to shear flow and die-lip throughput, while the high-molecular-weight fraction contributes to melt strength, bubble stability, and solid-state toughness. This resin is used on high-stalk blown film lines rather than cast film, blow moulding, or injection moulding lines. Processing conditions, mechanical property benchmarks, application scope, and regulatory boundaries are detailed below.
The HXM50100 designation belongs to the QAPCO Lotrene high-density polyethylene range and is characterized by a high-load melt index specification rather than a conventional low-load melt index. The low-load melt index at 2.16 kg is not the controlling specification for this molecular weight class; the relevant flow parameter is the high-load melt index of 10.0 g/10 min because the high-molecular-weight fraction raises the low-load viscosity beyond the range typically used for melt flow control. The bimodal chain architecture produces a shear-thinning curve that is flatter than that of a unimodal HDPE of equivalent HLMI. This rheological profile permits drawing of a stable high stalk after the die exit while retaining sufficient extensional viscosity to prevent bubble flutter and draw resonance. The density of 0.950 g/cm³ places the grade in the high-density class with a crystalline volume fraction sufficient to raise yield stress and reduce moisture permeability relative to linear low-density polyethylene, but the bimodal architecture partially offsets the reduction in impact toughness that would normally accompany this density in a unimodal resin.
In practice, the low-molecular-weight fraction functions as an internal processing aid during extrusion through the die land. The high-molecular-weight fraction controls the elastic memory of the melt and supports the high-stalk bubble configuration. The balance between these fractions affects die swell, melt fracture onset, and the orientation distribution in the final film. Lot-to-lot variation in molecular weight distribution is controlled by the polymerization and catalyst kinetics; converters should track high-load melt index, density, and film impact retention together because these values do not vary independently. Published data for the exact interrelationship between catalyst residue and stabilizer consumption in this specific grade are limited.
The operating envelope for HXM50100 is not defined solely by barrel setpoints. In high-stalk film production, the melt must remain below thermal degradation onset while remaining above the temperature at which the high-molecular-weight fraction relaxes sufficiently in the die. Melt temperature measured at the die exit is commonly held between 190°C and 210°C. Below 180°C, die-lip deposit, surface roughness, and melt fracture increase because long relaxation times prevent complete stress relaxation before the melt leaves the die. Above 220°C, oxidative chain scission becomes measurable even with the standard hindered phenolic stabilizer package; gel formation increases and dart impact retention in thin-gauge film declines. This window should be verified on the production line because thermocouple position, screw design, and residence time distribution can shift the actual melt temperature by 5°C to 10°C relative to setpoint.
Grooved-feed single-screw extruders with L/D 25:1 to 30:1 and screw diameters from 45 mm to 120 mm are preferred for this resin. The grooved feed section is critical because it generates the solids conveying pressure required to feed the high-molecular-weight polymer at stable output. Screw speed must be limited to control viscous shear heating. The die gap is typically set between 1.2 mm and 1.8 mm, and the blow-up ratio is normally between 3:1 and 5:1. Frost-line height is the main control for tear balance and stalk stability. A frost line that is too low reduces transverse orientation and can produce a wobbly bubble with gauge bands; a frost line that is too high increases film flatness variability and may overstretch the melt before crystallization. Air ring velocity, internal bubble cooling, and die temperature uniformity are therefore adjusted on a lot-specific basis rather than fixed by generic guidelines. Published data for the maximum stable output of HXM50100 on a given extruder configuration are limited; converter trials are required because the limiting factor is often bubble aerodynamics rather than resin rheology.
Thin-gauge T-shirt bags, loop-handle carrier bags, industrial liners, and waste sacks are typical conversion applications. Films blown in the 8 µm to 25 µm thickness range are common where a high strength-to-weight ratio is required. Dart drop impact energy per unit thickness is measured by ISO 7765-1 or ASTM D1709 Method A; tear resistance is measured by ASTM D1922 or ISO 6383-2. The choice of film thickness must be governed by end-use load and sealing geometry, not by resin alone. For heavy-duty sack liners, increasing gauge or blending with linear low-density polyethylene may be necessary. High-molecular-weight HDPE films of this class provide comparatively high tensile yield stress and moderate elongation to break; they do not provide the elastic recovery of an ethylene-vinyl acetate film or the clarity of a metallocene LLDPE blown film.
The values in the following table are representative of the bimodal high-molecular-weight high-density polyethylene grade class and should not be treated as lot-certification limits. The QAPCO certificate of analysis for each production lot is the controlling document. Film property values depend strongly on film thickness, die gap, frost-line height, and blow-up ratio; the values below are quoted from standard test specimens or controlled laboratory films unless otherwise noted.
| Property | Typical range | Unit | Test method |
|---|---|---|---|
| Nominal density at 23°C | 0.950 | g/cm³ | ISO 1183-1 |
| High-load melt index (190°C, 21.6 kg) | 10.0 | g/10 min | ISO 1133-1:2022 / ASTM D1238-13 Condition F |
| Tensile stress at yield | 23–25 | MPa | ISO 527-2 |
| Tensile strain at break | >600 | % | ISO 527-2 |
| Flexural modulus | 1000–1200 | MPa | ISO 178 |
| Vicat softening temperature | 126–128 | °C | ISO 306/A120 |
| Environmental stress crack resistance, F50 | >500 | h | ASTM D1693-15 Condition B |
| Dart drop impact, 25 µm laboratory film | 250–350 | g | ISO 7765-1 / ASTM D1709-15 Method A |
The environmental stress crack resistance test is particularly relevant for packaging of detergents, wet chemicals, or stressed filled sacks. The condition specified above uses 100% Igepal and a notched specimen; field performance also depends on film orientation, residual stress, and sealing conditions. The dart drop impact value should not be extrapolated directly from laboratory film to commercial film because gauge profile, die-gap-induced orientation, and frost-line height change energy absorption. Converters are advised to measure dart drop impact on production samples and to track lot-to-lot variability rather than relying on a single nominal value.
The primary difference from a conventional unimodal HDPE film grade of similar density is the distribution of molecular weight, not the average density. A unimodal resin may exhibit similar tensile yield stress but lower melt strength in high-stalk processing and lower environmental stress crack resistance. The bimodal distribution in HXM50100 allows a high-molecular-weight fraction to remain processable at conventional film extruder temperatures while still providing the extensional viscosity required for bubble stability. In contrast, a unimodal resin with the same high-molecular-weight fraction would require higher melt temperatures, which increases degradation risk, or lower throughput, which reduces economic viability.
Compared with butene linear low-density polyethylene at 0.918–0.922 g/cm³, HXM50100 exhibits higher density, higher tensile yield stress, higher flexural modulus, and lower moisture permeability per unit thickness. However, low-density LLDPE grades typically provide better dart drop impact and puncture resistance in thin films, particularly at low temperatures. HXM50100 should therefore be compared not as a direct impact-toughness substitute but as a stiff, creep-resistant layer where film strength and down-gauging are controlled by tensile yield and tear balance. Coextruded structures using HXM50100 as a high-density core or outer layer with an LLDPE or metallocene LLDPE sealing layer are common when both stiffness and hot-tack performance are required.
Within the QAPCO high-molecular-weight film product family, the practical differences are expressed through high-load melt index and density. A lower-HLMI grade of the same density would exhibit higher melt strength but would be more difficult to extrude at thin gauge without excessive melt temperature; a higher-HLMI grade would flow more readily but may show reduced bubble stability in high-stalk film. The 10.0 g/10 min high-load melt index of HXM50100 occupies a mid-range position suited to general carrier bag and industrial liner applications. Published data for direct comparative trials between HXM50100 and other specific QAPCO grades are limited; selection should be based on converter trials using the same die, air ring, and film gauge as the intended production campaign.
Regulatory compliance claims must be verified against the QAPCO product safety data sheet and the applicable food contact statement. HDPE olefin polymers of this density may be evaluated under FDA 21 CFR 177.1520(c) for direct food contact, subject to end-use extraction limits. For the European market, finished film must meet overall migration and specific migration conditions under Regulation (EU) No 10/2011; the resin is not automatically approved for all food types merely because it is an olefin polymer. REACH registration and SVHC status below 0.1 wt% should be confirmed from the supplier SDS. RoHS III compliance under Directive (EU) 2015/863 requires verification of lead, cadmium, mercury, hexavalent chromium, PBB, and PBDE concentrations in the finished article.
| Regulatory area | Relevant reference | Verification boundary |
|---|---|---|
| FDA food contact | 21 CFR 177.1520(c) | Finished film extraction limits and end-use conditions |
| EU food contact | Regulation (EU) No 10/2011 | Overall migration and specific migration limits |
| REACH | Directive 1907/2006/EC | SVHC concentration < 0.1 wt% per supplier SDS |
| RoHS III | Directive (EU) 2015/863 | Pb, Cd, Hg, Cr(VI), PBB, PBDE in homogeneous material |
For warehouse handling, the resin does not require predrying as a step to remove absorbed water of crystallization, but surface condensation on cold pellets in high-humidity storage can introduce microvoids in the film. If visible surface moisture is present, a hopper dryer at 70–80°C for 2 h is used before extrusion. Additive masterbatches should be screened for free-radical scavengers or excessive external lubricants because these can shift the stabilizer balance and increase die deposit formation. For food-contact structures, corona treatment should be limited to the dyne level required by the printing or lamination process; overtreatment can increase surface oxidation and may alter migration behavior. These boundaries are operational limits rather than resin defects and should be controlled in the converter quality plan.