| HS Code | 641533 |
| Melt Flow Rate | 0.05 g/10 min (190°C/2.16 kg) |
| Density | 0.954 g/cm³ |
| Tensile Strength At Yield | 26 MPa |
| Tensile Strength At Break | 32 MPa |
| Elongation At Break | >600% |
| Flexural Modulus | 1200 MPa |
| Vicat Softening Temperature | 125 °C |
| Heat Deflection Temperature | 75 °C (0.45 MPa) |
| Hardness Shore D | 65 |
| Environmental Stress Crack Resistance | >1000 h |
| Water Absorption | <0.01% |
| Melting Temperature | 130 °C |
| Crystallization Temperature | 115 °C |
| Volume Resistivity | >10^16 ohm·cm |
| Dielectric Constant | 2.3 |
As an accredited PTTGC HDPE INNOPLUS HD7000F factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | PTTGC HDPE INNOPLUS HD7000F is packaged in 25 kg polyethylene bags, stacked on 1,000 kg pallets for shipment. |
| Container Loading (20′ FCL) | Container loading (20′ FCL): PTTGC HDPE INNOPLUS HD7000F supplied in 25 kg bags, palletized, maximum 25 MT per container. |
| Shipping | PTTGC HDPE INNOPLUS HD7000F is a non-hazardous polyethylene resin, typically shipped in 25 kg bags or jumbo bags on pallets. Transport in clean, dry, covered containers or trucks. Store away from moisture, heat, direct sunlight, and contamination. Ensure packaging remains sealed and intact during transit. |
| Storage | Store PTTGC HDPE INNOPLUS HD7000F in a cool, dry, well-ventilated warehouse, away from direct sunlight, heat, flames, and strong oxidizers. Keep original bags/containers closed, palletized, and off the floor to prevent moisture and contamination. Avoid dust generation and static discharge. Use first-in, first-out stock rotation. Maintain ambient conditions; avoid prolonged UV exposure. Keep away from incompatible materials. |
| Shelf Life | PTTGC HDPE INNOPLUS HD7000F typically has a 24-month shelf life when stored unopened, cool, dry, ventilated, away from direct sunlight. |
The conversion of HD7000F on high-stalk upward blown film lines for retail carrier bag stock begins with a nominal melt flow rate of 0.04 g/10 min at 190 °C under 2.16 kg as determined by ISO 1133-1:2022, and a nominal density of 0.950 g/cm³ under ISO 1183-1:2019. On a 75 mm grooved-feed single-screw extruder with 30:1 L/D and an 1100 mm annular die with 1.8 mm die gap, the resin is processed at a barrel profile of 180–220 °C and a die temperature of 200–215 °C, with a blow-up ratio of 3.5:1 to 4:1 and a frost-line height maintained at 5–7 die diameters. The formulation for retail bag film is 100% HD7000F; a PE-based slip/antiblock masterbatch is added at 0.5–1.5 wt%, and when dart impact at 25 μm gauge falls below the converter's target, up to 20 wt% LLDPE may be incorporated. Mechanical compliance testing follows ASTM D882 tensile, ASTM D1709 dart impact, and ASTM D1922 Elmendorf tear; surface wetting tension is evaluated under ASTM D2578 with a target of 38–42 mN/m. Downstream conversion uses servo-driven bag machines operating at 250–350 forming cycles per minute. Terminal product types include T-shirt carrier bags, perforated roll bags, and thin produce bags. Batch-to-batch high-load melt index variation on 1100 mm die lines can shift the frost-line position by ±50 mm; air-ring airflow adjustment is preferred over barrel temperature changes because the latter destabilizes the bubble for at least 15–20 min. Operational boundary: if the die gap is reduced below 1.6 mm at 150 kg/h, melt pressure at the breaker plate may exceed 35 MPa and produce shutter marks; the specified die gap is treated as the lower processing limit.
In refuse sack extrusion, the formulation boundary is not set by neat HD7000F but by the acceptable reduction in ASTM D1709 dart impact when post-consumer HDPE flake or pelletized recyclate is introduced. The base resin may be run at 100% HD7000F, or a dosing side feeder may add 10–15 wt% washed post-consumer HDPE at the throat; recycled content above 20 wt% typically requires a line-speed reduction of 8–12% to maintain tear resistance under ASTM D1922 and to prevent film splits at the collapsing frame. Compliance for municipal refuse sack stock frequently references tensile strength and elongation measured by ISO 527-3, puncture resistance by ASTM D5748, and dart impact by ASTM D1709 Method A at 25–50 μm nominal gauge. Extrusion equipment for high-output refuse film consists of a 90 mm grooved-feed single-screw extruder with 30:1 L/D, an internal bubble cooling system, and an 1800 mm die with 2.0 mm die gap. Melt temperature is held at 200–225 °C, with blow-up ratio at 4:1 to 5:1 and frost-line height at 8–10 die diameters for high-stalk geometry. Terminal films include star-sealed refuse sacks, drawstring waste liners, and retail bin liners. Operational boundary: recycled flake with a bulk density below 0.45 g/cm³ causes feed bridging in smooth-bore throats; a grooved-feed section with forced feeding is required.
For industrial heavy-gauge liners above 100 μm nominal thickness, grooved-feed extrusion of HD7000F shifts from fracture-limited to back-pressure-limited operation. The high molecular weight that supports melt strength also raises head pressure; on a 120 mm extruder running 180 kg/h at a die gap of 2.3 mm, pressure at the screen changer is maintained below 28 MPa by using a 60 mesh screen over a 40 mesh breaker, with screen changes scheduled every 6–8 h when process regrind is blended at 15 wt%. The formulation for this segment is 85–100% HD7000F with 0–15 wt% internally generated edge-trim regrind; carbon black masterbatch is added at 2.0–3.0 wt% when ultraviolet resistance is required for outdoor exposure. Industry compliance standards include ASTM D4976-22 for polyethylene molding and extrusion materials, ASTM D882 tensile, ASTM D1709 dart impact, and ASTM D1922 tear; for temporary liner applications, puncture resistance is tested under ASTM D4833. The downstream process is high-stalk upward blown film with a 3:1 to 4:1 blow-up ratio and a frost-line height set at 6–8 die diameters; edge trim is fed back after grinder densification to maintain consistent bulk density. Terminal product types include heavy-duty industrial refuse liners, construction debris sacks, and temporary concrete-curing films. Operational boundary: regrind addition above 15 wt% increases melt-pressure fluctuation by more than ±1.5 MPa at constant screw speed, producing visible gauge bands unless a continuous melt pump is installed.
Blown film based on HD7000F is considered for dry-food pouch liners only when the stabilizer package and the neat resin are confirmed to comply with EU 10/2011/EC Annex I and Annex II and with 21 CFR 177.1520(c) for olefin polymers in contact with aqueous and dry food types under the applicable extractive limits. The formulation in this segment is 100% virgin HD7000F; a food-grade antioxidant/carrier masterbatch is dosed at 0.2–0.4 wt%, and post-consumer recyclate is excluded to preserve migration-test validity. Extrusion is performed on a 70 mm grooved-feed blown-film line with 30:1 L/D, a 1600 mm die with 1.8 mm die gap, and a melt temperature of 190–215 °C to limit oxidative degradation and odor development. Blow-up ratio is held at 3:1 to 3.5:1; the frost-line height is 5–6 die diameters. Corona treatment to 38–42 mN/m under ASTM D2578 is applied before lamination or flexographic printing. Mechanical compliance testing follows ISO 527-3 tensile, ASTM D882 thickness-corrected tensile, ASTM D1922 tear, and ASTM D1894 coefficient of friction. Terminal product types include dry-food pouch inner liners, cereal box inner bags, and bakery paper overwrap films. Operational boundary: if the film is stored above 60% relative humidity and subsequently printed, surface moisture may reduce corona retention; the roll must be conditioned for 8 h at 35 °C before lamination.
When a converter evaluates down-gauging from a 50 μm LLDPE sealant web to a 35 μm HD7000F web, the substitution is governed by the ratio of secant modulus values rather than by tensile strength alone. HD7000F at a density of 0.950 g/cm³ exhibits a higher ASTM D882 secant modulus than a 0.920 g/cm³ LLDPE; therefore the thinner HD7000F web can maintain comparable buckling resistance in paper-like overwrap applications if the die gap and blow-up ratio are rebalanced. The production process for this stiffness-critical segment uses a 60 mm high-stalk blown-film line with 28:1 L/D, a 1.2 mm die gap, and a blow-up ratio of 4:1 to 5:1. Formulation addition comprises 90–100% HD7000F and 0–10 wt% HDPE-compatible processing aid masterbatch; LLDPE is not added in this segment because a 10 wt% LLDPE addition reduces secant modulus enough to nullify the down-gauging objective. Compliance testing uses ISO 527-3 tensile modulus, ASTM D882 elongation at break, and ASTM D1922 tear resistance; optical properties are measured under ASTM D1003 haze and ASTM D2457 gloss where surface appearance matters. Terminal product types include paper-like envelope films, protective overwrap for textile rolls, and lamination bases for flexible packaging. Operational boundary: at a blow-up ratio above 5:1 the high-stalk bubble becomes unstable under lateral air currents below 0.5 m/s; an enclosed calibration cage is required. Published dart impact and secant modulus values for this specific HD7000F-to-LLDPE down-gauging comparison are limited, so the substitution must be confirmed by line trials using the converter's own frost-line control and edge-gauge profile.
In coextruded packaging structures, HD7000F is assigned to the core layer rather than the sealant skins because its density of 0.950 g/cm³ under ISO 1183-1:2019 raises the bending stiffness of the total web without increasing the seal initiation temperature of the outer LLDPE skins. A typical three-layer formulation for a 70 μm film is 20% LLDPE skin / 60% HD7000F core / 20% LLDPE sealant, with compatibility maintained within the polyethylene family; no adhesive tie layer is required when the skins are LLDPE or LDPE. Coextrusion equipment uses a three-layer annular die of 1600 mm diameter, 1.8 mm total die gap, and three extruders—a 90 mm core extruder and two 45 mm skin extruders—with a core melt temperature of 200–220 °C and skin temperatures 15–20 °C lower. The bubble runs at a blow-up ratio of 3:1 to 4:1; layer stability is monitored by capacitance gauge scanning every 50 mm across the web. Compliance for the final coextruded film follows ISO 527-3 tensile, ASTM D1876 interlaminar adhesion, and ASTM D1003 haze. Terminal product types include stiff overwrap for bundled goods, lamination substrates for paper-plastic structures, and hygiene product packaging films. Operational boundary: if the core layer exceeds 70 wt% of the total structure, the bubble may exhibit asymmetric quench stress and web curl; in such cases the die is rotated at 1–2 rpm to randomize thickness variation.
Competitive PTTGC HDPE INNOPLUS HD7000F prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
A polymer identification block for PTTGC HDPE INNOPLUS HD7000F identifies the resin as a high molecular weight, bimodal high-density polyethylene intended for blown film extrusion. The nominal density is 0.950 g/cm³ when measured by ISO 1183-1, and the nominal melt mass-flow rate is 0.04 g/10 min at 190 °C under a 2.16 kg load by ISO 1133-1:2022, procedure A. The bimodal molar mass distribution combines a high molecular weight fraction for melt strength with a lower molecular weight fraction that improves shear thinning; on production blown film extruders this permits bubble architecture that resists draw resonance during low-tension take-off. The resin is stabilized with a hindered phenolic antioxidant and a phosphite processing stabilizer, and the pellet geometry is cylindrical to promote consistent feeding in grooved-feed extruders rather than in minimal-vent smooth-bore hopper systems. The product is not characterized by a single melt flow index alone; shear sensitivity and extensional viscosity must be considered when changing from monomodal HDPE or LLDPE film grades.
| Property | Test method | Nominal value |
|---|---|---|
| Melt mass-flow rate, 190 °C, 2.16 kg | ISO 1133-1 | 0.04 g/10 min |
| Density, 23 °C | ISO 1183-1 | 0.950 g/cm³ |
| Melting peak, DSC | ISO 11357-3 | 131 °C |
| Tensile yield strength, MD | ISO 527-3 | 25 MPa |
| Tensile elongation at break, MD | ISO 527-3 | 500 % |
| Elmendorf tear resistance, TD | ISO 6383-2 | 40 g |
| Dart drop impact, F50 | ISO 7765-2 | 160 g |
| Film haze | ISO 14782 | 85 % |
The values in the table are manufacturer-published nominal values for resin and 25 µm blown film produced at a 4:1 blow-up ratio and a 1.4 mm die gap. They are not specification limits and should not be used for lot acceptance without reference to the certificate of analysis.
Bubble stability with HD7000F derives from the chain entanglement density associated with the high molecular weight fraction; however, the same architecture imposes equipment requirements. On a 65 mm grooved-feed blown film extruder with 30:1 L/D and a 250 mm spiral mandrel die, the melt temperature measured at the adapter is typically controlled between 190 °C and 220 °C to avoid excessive back pressure and to stabilize the frost-line height. The die gap should not be reduced below 1.2 mm without a corresponding increase in blow-up ratio and cooling air velocity; below this threshold, shear rates can exceed the critical level for melt fracture and produce orange-peel surface defects. Recommended blow-up ratios range from 3.5:1 to 5:1, and the frost-line height is controlled to 6 to 8 die diameters to balance machine-direction and transverse-direction orientation. At melt temperatures above 230 °C, oxidative degradation of the high molecular weight chains can initiate; the practical upper continuous operating limit is therefore 225 °C at the adapter.
Rheological characterization at 190 °C by rotational and capillary rheometry typically shows a low-frequency complex viscosity that is higher than medium molecular weight film grades, while the power-law shear-thinning index is comparable to broad-MWD HDPE. On small-scale blown film lines, the measured die pressure can exceed 250 bar when the die gap is below 1.2 mm at high screw speeds; this pressure must be checked against the die manufacturer’s mechanical rating. A spiral mandrel die with a relaxed spiral clearance and generous flow-channel depth is preferred to distribute the high-viscosity melt evenly without dead spots. In thin-film operations, the limiting factor is usually bubble cooling rather than plastication. At a target thickness of 12 µm, cooling air flow and collapsing geometry must bring the film below the crystalline solidification temperature before the nip; otherwise blocking and uneven web tension occur at the winder. Melt temperatures of 200–215 °C with external cooling air at 10–18 °C allow stable production speeds up to the mechanical limit of the downstream bag-welding line. The resin should not be dry blended with high-MFR peroxide masterbatches intended for polypropylene viscosity control; uncontrolled radical generation in HDPE produces crosslinked gel particles that appear as pinholes in films below 15 µm.
For ultra-thin carrier bag conversion on high-speed side-weld machines, film manufactured from HD7000F is typically extruded at 10–15 µm and evaluated using ISO 527-3 for tensile properties, ISO 7765-2 for dart drop impact, and ISO 6383-2 for tear resistance in the machine and transverse directions. The high molecular weight main fraction and controlled comonomer distribution raise the yield stress relative to conventional blown film grades, permitting draw-down without immediate strain whitening at the bag handle perforation. In production-scale side-weld bag conversion, the critical defects are handle tear propagation at the weld boundary and film blocking on the unwind stand; both are minimized by maintaining a film density near 0.950 g/cm³ and by using the resin’s additive package. The material is also run on T-shirt bag lines where the film is folded, punched, and sealed in a continuous rotary motion; the melt strength allows short neck-height operation during rapid production rate changes without bubble sag. Because the resin is a high-density polyethylene, the film develops a crystalline lamellar structure during air-ring cooling; the balance of blast air temperature and line speed therefore controls dart impact beyond the resin’s intrinsic value. If the film is quenched too rapidly, transverse orientation increases and dart impact can fall below the value required by bag-drop tests. Conversely, if the film is cooled too slowly, blocking at the collapsing frame increases and the reel can telescope during winding. The practical operating window for a 25 µm film is therefore defined by a frost-line height that is neither too low nor too high, usually between 100 mm and 300 mm above the air ring on a 250 mm die, depending on ambient humidity and air temperature.
When HD7000F is compared with a conventional medium molecular weight HDPE film resin having a melt flow rate of 0.7–1.2 g/10 min, the low nominal melt flow rate of 0.04 g/10 min does not fully describe extrudability; the broader molecular weight distribution of the bimodal product provides greater shear thinning at extrusion shear rates while retaining low-shear melt strength for bubble stability. In film evaluations, the high molecular weight HDPE shows higher dart drop impact and transverse-direction tear resistance, whereas the medium-MFR monomodal HDPE can exhibit lower back pressure and higher throughput at the same screw speed but a narrower stable bubble window. Against linear low-density polyethylene, HD7000F produces higher modulus and lower intrinsic impact strength, making it unsuitable as a drop-in replacement for LLDPE stretch-film or heavy-duty packaging. However, the HDPE grade reduces film blocking and allows lower film thickness without losing bag-opening stiffness.
| Parameter | HD7000F | Medium-MFR HDPE film grade | LLDPE film grade |
|---|---|---|---|
| Melt mass-flow rate | 0.04 g/10 min | 0.8 g/10 min | 1.0 g/10 min |
| Density | 0.950 g/cm³ | 0.958 g/cm³ | 0.920 g/cm³ |
| Film modulus | 900 MPa | 1100 MPa | 250 MPa |
| Dart drop impact, F50 | 160 g | 100 g | 300 g |
| Stable die gap range | 1.2–1.8 mm | 0.9–1.4 mm | 0.8–1.2 mm |
| Melt temperature range | 190–220 °C | 180–210 °C | 190–240 °C |
The comparison is not intended for direct formula substitution because the screw geometry, air ring, and die gap must be selected for the specific resin. When changing from a medium-MFR HDPE to HD7000F, operators should increase the die gap by 0.2–0.4 mm and verify that the extruder drive has sufficient torque for the higher melt viscosity. If the line is equipped with a barrier screw designed for LLDPE, the feed section may overheat due to higher energy dissipation; a grooved-feed HDPE screw is preferred. The differentiation also appears in screw design. A conventional polyolefin barrier screw with a feed zone, barrier section, and mixing section may be adequate for medium-MFR HDPE, but the high molecular weight fraction of HD7000F requires a grooved-feed section to maintain solids conveying and to prevent feed surging. Screws with an L/D ratio below 24:1 can produce unmelts and pressure fluctuations when operating at low melt temperatures. In direct film substitution, the extruder should be capable of maintaining a specific energy input of at least 0.25 kWh/kg to avoid unmelts, although actual specific energy depends on screw speed, temperature profile, and die restriction.
Certificate of analysis documentation for HD7000F typically reports melt flow rate, density, pellet appearance, and contamination ratings for each production lot. Incoming-resin verification should include melt flow rate by ISO 1133-1 and density by ISO 1183-1; if the resin is intended for food-contact applications, the converter must confirm compliance under European Commission Regulation (EU) 10/2011 and FDA 21 CFR 177.1520 because the final additive composition and film fabrication conditions influence overall packaging compliance. The product is not a universal grade for injection molding or pipe extrusion; its low melt flow rate and high melt viscosity restrict flow into thin-wall injection tools and require high torque in single-screw extruders designed for film. Under REACH Regulation (EC) 1907/2006, the grade is supplied with a safety data sheet that identifies any residual monomers or process aids present above reporting thresholds. The converter must evaluate the final article under the packaging and packaging waste directive 94/62/EC if the film is used for secondary or tertiary packaging. No statement is made here concerning direct food-contact approval; such determinations require migration testing under the applicable simulant conditions described in EU Regulation 10/2011 or FDA 21 CFR 177.1520 and are the responsibility of the final article manufacturer.
Operationally, HD7000F should be purged with a lower-MFR HDPE or a commercial purging compound before extended shutdowns; retained molten resin in the die or adapter that remains above 180 °C for more than 20 min can generate crosslinked gel. Avoid blending with polypropylene or random copolymer PP because the incompatible interface creates delamination in thin films. If edge-trim regrind is returned to the feed, it should be dried to below 0.05 % moisture and limited to 20 wt% of the total feed to preserve bubble stability and film toughness. These limits reflect film-line observations and should be revalidated with the specific extruder screw profile, die diameter, and air-ring geometry.