| HS Code | 362600 |
| Density | 1.31 g/cm³ |
| Water Absorption 24 H | 0.08% |
| Tensile Strength | 55 MPa |
| Tensile Elongation At Break | 15% |
| Flexural Strength | 85 MPa |
| Flexural Modulus | 2400 MPa |
| Charpy Notched Impact Strength | 2.5 kJ/m² |
| Rockwell Hardness | M75 |
| Deflection Temperature Under Load 1 8 Mpa | 65 °C |
| Deflection Temperature Under Load 0 45 Mpa | 150 °C |
| Melting Point | 224 °C |
| Molding Shrinkage Flow Direction | 1.5-2.0% |
| Volume Resistivity | 1E16 Ω·cm |
| Dielectric Strength | 18 kV/mm |
| Arc Resistance | 120 s |
| Ul94 Flammability Rating | V-0 (0.75 mm) |
As an accredited Polyplastics DURANEX® Unreinforced FR PBT 201NF factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Packaged in 25 kg moisture-resistant bags, palletized for shipment, each containing DURANEX® Unreinforced FR PBT 201NF resin. |
| Container Loading (20′ FCL) | Polyplastics DURANEX® 201NF unreinforced FR PBT loaded in 20′ FCL dry container, palletized bags, secured for export shipment. |
| Shipping | DURANEX® Unreinforced FR PBT 201NF is typically shipped as non-dangerous PBT resin pellets in sealed moisture-barrier packaging. Keep dry and away from heat, sunlight, and ignition sources. Verify SDS, packaging, labeling, and local/international transport regulations before shipment. |
| Storage | For DURANEX 201NF PBT, store in original closed containers in a cool, dry, well-ventilated area protected from sunlight, heat, moisture and ignition sources. Keep away from strong oxidizers and incompatible chemicals. Avoid dust generation and static buildup. Maintain good housekeeping and use grounded equipment. Follow local regulations and the manufacturer’s SDS. Do not store near food or drink. |
| Shelf Life | For DURANEX 201NF, store dry and cool away from sunlight; shelf life is typically two years from manufacture in unopened packaging. |
Competitive Polyplastics DURANEX® Unreinforced FR PBT 201NF prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Polyplastics DURANEX® 201NF is an unreinforced flame-retardant polybutylene terephthalate (PBT) injection-moulding compound specified for electrical insulation components that require a UL 94 V-0 flammability rating at a minimum wall thickness of 0.75 mm without the anisotropic shrinkage, warpage, and abrasive wear associated with glass-fibre-reinforced PBT. The base resin is a semicrystalline thermoplastic polyester in which the flame-retardant system raises melt viscosity sensitivity and density relative to standard unfilled PBT; the grade designation does not identify the flame-retardant chemistry, and lot-specific documentation must be consulted for halogen content, antimony synergist presence, extractables, and comparative tracking index certification. The material is supplied as pelletised feedstock and is designated PBT-FR under ISO 11469.
Principal end-uses include thin-wall connectors, relay bases, terminal blocks, switch covers, coil bobbins, circuit-breaker housings, and sensor enclosures. In these applications the material is selected because its unreinforced structure allows lower melt pressure, improved thin-wall filling, better knit-line appearance, and reduced tool wear compared with 30% glass-fibre-reinforced FR PBT, while retaining a flame-retardant classification sufficient for unattended electrical devices. Published data for this specific configuration is limited to the manufacturer’s current technical data sheet; the values below are representative of unreinforced FR PBT and should be confirmed against the current grade-specific datasheet before lot acceptance.
| Property | Test method | Typical value |
|---|---|---|
| Density | ISO 1183-1 | 1.46 g/cm³ |
| Tensile stress at yield | ISO 527-1/-2 | 55 MPa |
| Tensile elongation at break | ISO 527-1/-2 | 6 % |
| Flexural modulus | ISO 178 | 2600 MPa |
| Flexural strength | ISO 178 | 85 MPa |
| Charpy notched impact strength, 23 °C | ISO 179-1/1eA | 4 kJ/m² |
| Heat deflection temperature, 1.80 MPa | ISO 75-1/-2 | 65 °C |
| Heat deflection temperature, 0.45 MPa | ISO 75-1/-2 | 150 °C |
| Melt volume-flow rate, 250 °C/2.16 kg | ISO 1133-1:2022 | 20 cm³/10 min |
| Water absorption, 24 h/23 °C | ISO 62 | 0.08 % |
| Dielectric strength, 1 mm plaque | IEC 60243-1 | 18 kV/mm |
| Volume resistivity | IEC 62631-3-1 | 1 × 10¹⁴ Ω·m |
| Comparative tracking index | IEC 60112 | 250 V |
| Flame retardancy | UL 94 / IEC 60695-11-10 | V-0 at 0.75 mm |
| Mould shrinkage, flow direction | ISO 294-4 | 1.6–2.0 % |
These values are not automatic lot-release specifications. Incoming quality control should rely on the supplier’s certificate of analysis and on moulded plaques or end-use parts evaluated under the relevant ISO or ASTM procedure because laboratory specimen values can diverge from moulded-part behaviour in thin walls, weld lines, and areas of high orientation.
The failure mode is not a simple reduction in stiffness. In a 30% glass-fibre-reinforced FR PBT, the fibre network raises flexural modulus to approximately 8000–9000 MPa and reduces isotropic shrinkage to 0.3–0.8%, but it also creates flow-induced fibre orientation. In thin-wall connector housings with adjacent wall sections of 0.4 mm and 1.0 mm, differential fibre alignment can produce out-of-plane warpage after ejection and lead to contact misalignment. DURANEX 201NF, as an unreinforced system, exhibits flexural modulus in the 2500–2800 MPa range and higher mould shrinkage, typically 1.5–2.0%; the shrinkage is more uniform between flow and transverse directions, which reduces thermally induced internal stress gradients. The trade-off is that thin ribs and snap-fit features must be designed with lower load-bearing capacity and higher creep compliance than would be acceptable in glass-filled PBT. Tensile stress at yield for unreinforced FR PBT is typically 55–60 MPa, compared with 120–140 MPa for a 30% glass-filled FR grade, and Charpy notched impact strength remains in the 3–5 kJ/m² range rather than the 8–12 kJ/m² range seen in many reinforced grades.
These differences require revised gate location, wall-thickness distribution, and ejection design. The lower viscosity of the unreinforced grade allows filling at lower injection pressure, but the higher mould shrinkage requires larger core and cavity dimensions. In multi-cavity tools, the moulder should expect greater cavity-to-cavity mass variation if runner balance is not adjusted, because the flame-retardant system reduces thermal stability at the upper end of the melt-temperature range. Sharp internal corners should be avoided in snap-fit arms and latch features; a minimum radius of 0.5 mm is recommended to reduce notch sensitivity and stress concentration.
Pre-drying is mandatory. DURANEX 201NF should be dried with a desiccant-bed dryer at 120 °C for 4 h to 6 h, with a dew point no higher than −30 °C; residual moisture in the pellets should be held below 0.02%. At ambient relative humidity above 60%, hopper residence time should be restricted because moisture reabsorption in PBT can hydrolyse the polyester backbone during plastication, reducing molecular weight and producing a viscosity drop and a loss of tensile elongation. The melt temperature should be maintained between 240 °C and 260 °C measured at the nozzle. The barrel should be purged if melt temperature exceeds 270 °C for more than 5 min; prolonged residence time at high temperature can cause flame-retardant degradation, discolouration, silver streaking, and mould deposits.
Barrel profile settings from feed throat to nozzle are typically 230 °C, 240 °C, 250 °C, 250 °C, and 255 °C. A general-purpose screw with an 18:1 to 22:1 L/D ratio and low-to-medium compression ratio of 2.0:1 to 2.5:1 is adequate. A reverse-taper check valve or ball-type check valve should be used with retracted pullback of 3–5 mm to prevent decompression-related air entrapment. Back pressure should be 0.3–1.0 MPa; higher back pressure increases melt residence time and shear heating. Injection speed should be medium to high for thin-wall filling, but holding pressure and gate freeze time must be calibrated because unreinforced PBT solidifies faster than glass-filled PBT at low wall thickness. Mould temperature should normally be 40–80 °C; higher mould temperatures improve surface gloss and weld-line strength but increase cycle time and mould shrinkage variability.
Unreinforced PBT crystallises rapidly from the melt; therefore, mould temperature and holding pressure must control warpage rather than slow cooling. If the mould surface temperature is below 40 °C, quench-induced crystallinity gradients can produce sink marks and differential shrinkage across changes in wall thickness. A mould temperature of 60–80 °C generally increases crystallinity and dimensional stability, but cycle time increases and ejection may require additional draft because shrinkage over the core is higher. Flame-retardant PBT compounds often generate volatile decomposition products that condense on mould surfaces. Vents should be placed at the end of fill and along weld lines; a vent depth of 0.01–0.03 mm is typical for unfilled PBT. Periodic cleaning of the vent channels prevents gas-burn marks and short shots. Use of mould release agents is generally unnecessary and may worsen plate-out.
In cavity pressure terms, thin-wall unreinforced PBT components often reach end-of-fill cavity pressure in the 30–60 MPa range. Clamp force should be calculated from projected area and cavity pressure with a safety factor of 1.3–1.5. For a multi-cavity hot-runner tool, thermocouple placement in each drop and individual tip control reduce imbalance that causes flash or sink marks. Holding pressure should be reduced only after gate freeze is confirmed by weight stabilisation; otherwise moulded-part mass varies and shrinkage can drift across the production run.
In sealed or low-ventilation switchgear, thermal ageing of flame-retardant systems can release low-molecular-weight species that migrate to metal contacts and increase contact resistance. For DURANEX 201NF, the relevant operational boundary is the continuous-use temperature and the outgassing limit of the finished assembly. The processor should verify contact compatibility by exposing moulded parts in a heated enclosure at 85 °C or 105 °C for 1000 h according to the device qualification plan. The current UL Yellow Card may list relative thermal index values, but these are not direct guarantees against contact resistance drift. If the application involves sealed relays or hermetically enclosed connectors, the manufacturer should be consulted for extractables data and for the recommended maximum continuous-use temperature.
Electrical tracking performance is evaluated under IEC 60112; unreinforced FR PBT grades of this class typically fall in the 250 V or 175 V comparative tracking index range depending on formulation. This value affects creepage distance calculations in printed-circuit-board terminal blocks. The moulded part should not be combined with amine-based additives, strongly alkaline cleaning agents, or hot mineral acids because PBT hydrolyses under alkaline and strongly acidic conditions at elevated temperatures. In mineral-insulated or oil-filled devices, long-term oil resistance and additive extraction should be evaluated because plasticiser migration from elastomeric seals can alter the flame-retardant system and reduce mechanical strength.
| Requirement | Standard or regulation | Typical status |
|---|---|---|
| Flammability classification | UL 94 / IEC 60695-11-10 | V-0 at 0.75 mm |
| Comparative tracking index | IEC 60112 | 250 V or 175 V depending on lot |
| Restriction of hazardous substances | RoHS Directive 2011/65/EU as amended by (EU) 2015/863 | Supplier conformance declaration required |
| REACH SVHC | Regulation (EC) No 1907/2006 | Supplier declaration required |
| Density | ISO 1183-1 | 1.45–1.50 g/cm³ |
| Tensile property | ISO 527-1/-2 | 55–60 MPa at yield |
| Melt flow rate | ISO 1133-1:2022 | 15–25 cm³/10 min at 250 °C/2.16 kg |
| Mould shrinkage | ISO 294-4 | 1.5–2.0 % |
Within the DURANEX FR family, an unreinforced grade is selected when the part requires lower anisotropic warpage and a higher-gloss surface rather than structural load-bearing capacity. Reinforced FR PBT grades, such as glass-filled or glass/mineral-filled, are specified when the component must survive elevated mechanical stress at heat deflection temperatures approaching 150 °C or higher, but they require larger gate diameters, higher injection pressures, and post-mould annealing to control warpage. Compared with general-purpose unfilled PBT, DURANEX 201NF shows higher density, lower tensile elongation, and a narrower processing window because the flame-retardant package affects nucleation rate and crystallisation behaviour. These differences are not categorical but should be quantified for the specific part geometry under ISO 294-4 shrinkage evaluation and ISO 527-1/-2 tensile testing.
For high-volume connector production, the principal processing failures observed on conventional injection moulding machines are gate blush caused by excessively fast injection, vent-related burn marks at the end of fill, and plate-out on core pins after extended runs. The use of a dedicated barrel and screw with low-shear mixing is preferred because residue from previous high-temperature resins, especially polysulfones or polyetherimides, can generate black specks or delamination in unreinforced FR PBT. When changing from a glass-filled grade to DURANEX 201NF, the barrel and hot runner should be purged with a commercial purging compound followed by unreinforced PBT to remove glass residues that would otherwise abrade the check ring and alter shot size consistency.