| HS Code | 418120 |
| Polymer Base | PBT |
| Glass Fiber Content | 40% |
| Hydrolysis Resistance | Hydrolysis-resistant grade |
| Density | 1.62 g/cm³ |
| Tensile Strength | 135 MPa |
| Tensile Elongation At Break | 2.0% |
| Flexural Modulus | 11,000 MPa |
| Flexural Strength | 200 MPa |
| Charpy Notched Impact Strength | 6 kJ/m² |
| Heat Deflection Temperature At 1 8 Mpa | 205 °C |
| Water Absorption | 0.07% |
| Mold Shrinkage | 0.2–0.8% |
| Coefficient Of Linear Thermal Expansion | 2–8 × 10⁻⁵ /°C |
| Volume Resistivity | 1 × 10¹⁶ Ω·cm |
| Dielectric Strength | 20 kV/mm |
| Flammability | HB |
As an accredited Polyplastics DURANEX® PBT+GF40%-Hydrolytic 7340 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Polyplastics DURANEX® PBT+GF40%-Hydrolytic 7340 is supplied in 25 kg moisture-proof bags, typically palletized with 40 bags per pallet. |
| Container Loading (20′ FCL) | Container Loading (20′ FCL): Polyplastics DURANEX® PBT+GF40%-Hydrolytic 7340 loaded palletized in moisture-proof bags, securely stowed for ocean freight. |
| Shipping | Polyplastics DURANEX® PBT+GF40%-Hydrolytic 7340 is typically shipped as non-hazardous polymer pellets in sealed moisture-barrier packaging. Keep dry, cool, covered, and protected from contamination, direct sunlight, and high humidity. Follow the SDS, local transport regulations, and maintain package integrity during handling. |
| Storage | Store DURANEX® PBT+GF40%-Hydrolytic 7340 in a cool, dry, well-ventilated area, away from direct sunlight, heat, moisture, and incompatible chemicals. Keep in sealed original packaging, palletized off the floor, and protect from humidity. Avoid moisture absorption before processing. Do not expose to open flames or excessive temperatures. Observe SDS, local regulations, first-in-first-out rotation, and recommended shelf life. |
| Shelf Life | Typical shelf life is 12–24 months when stored unopened in a dry, cool place, protected from moisture and direct sunlight. |
Competitive Polyplastics DURANEX® PBT+GF40%-Hydrolytic 7340 prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Polyplastics DURANEX® 7340 is a hydrolysis-stabilized polybutylene terephthalate injection-moulding grade reinforced with 40% glass fibre by mass. The designation identifies a high-modulus PBT compound intended for parts that must retain dimensional stability and load-bearing capacity after prolonged contact with hot water, ethylene glycol–water coolant, or high-humidity air. It is not a direct substitute for standard 30% glass-filled PBT or unfilled PBT; the higher fibre fraction and the hydrolysis control package alter rheology, mould shrinkage, weld-line formation, and thermal stability. The material is normally processed after desiccant drying to a residual moisture of ≤0.02%. Typical drying conditions for PBT are 120 °C for 4–6 h at a dew point of -35 °C or lower. Published data for this specific configuration is limited; therefore, the supplier’s certificate of analysis should be used to confirm lot-specific moisture content and melt viscosity before production start-up.
The primary degradation mechanism in hot-water service is autocatalytic ester hydrolysis. Water ingress in PBT occurs predominantly through amorphous regions; the ester linkage undergoes scission, producing carboxyl end-groups that reduce local pH and accelerate further chain scission. The hydrolysis rate is controlled by temperature, water activity, initial carboxyl concentration, and the effectiveness of the stabilizer package. In standard glass-filled PBT, the tensile-strength half-life at 85 °C and 85% RH can be less than 1,000 h; hydrolysis-stabilized grades are formulated to shift the half-life upward by modifying acid-end-group concentration or by chain extension. Fibre sizing can also influence this because the fibre–matrix interface acts as a preferential water pathway when sizing is not chemically bonded to the PBT matrix.
For 40% glass-fibre PBT, the high fibre fraction stiffens the part but also creates additional orientational boundaries. Tensile modulus measured by ISO 527-2 for 40% glass-reinforced PBT generally sits in the range 12,000–14,500 MPa, compared with 9,500–11,000 MPa for a 30% glass grade. This modulus increase is substantial but does not by itself guarantee hydrolytic resistance. The relevant comparative test is mechanical property retention after pressurised hot-water or coolant exposure, not the initial modulus. Screening should therefore include tensile specimens conditioned according to ISO 527-1/-2, followed by ageing in a sealed pressure vessel at 120 °C and then tested at 23 °C after redrying.
The additive chemistry used for hydrolysis resistance can also narrow the melt-processing window. Some hydrolysis stabilizers are active as acid scavengers or chain extenders during melt processing; excessive melt temperature or extended residence time can consume the active sites before the part enters service. The practical melt temperature for processing DURANEX® 7340 should be held at 250–270 °C, and barrel residence time above 270 °C should be limited to 5 min. The upper boundary is more stringent than for many standard PBT grades because additive degradation at the hot-runner manifold can reduce long-term performance even when unfilled PBT would survive the same thermal history. The fibre interface is not passive. Moisture uptake can be accelerated along fibre–matrix debonding cracks; hydrolytic ageing then combines chemical chain scission with physical fibre–matrix separation. That is why tensile modulus may remain high even as elongation at break drops, and why notched impact strength is an early failure indicator in wet-aged parts.
In underhood coolant valves, thermostat housings, and EGR cooler flanges, the material must retain clamp load after thermal cycling and hot coolant exposure. Moulded components on a 160 t hydraulic clamp with a 40 mm screw require a shot cushion of 3–6 mm and screw recovery speeds of 80–100 min⁻¹ to maintain fibre-length retention and avoid dead spots in the check ring. Weld lines located near sealing surfaces are a failure risk because fibre orientation across a weld line is nearly transverse; subsequent hydrolysis can attack the weld-line region preferentially. Mould filling simulation should be used to place weld lines away from the inner seal bead, and gas venting at the end of fill is required to prevent burning at the high cavity pressures used for 40% glass-filled PBT.
Hydrolysis-resistant PBT-GF40 is typically evaluated against standard PBT-GF30 and standard PBT-GF40 using dry as-moulded data and then after moisture ageing. The table below shows representative class-level property envelopes at 23 °C/50% RH. Where the supplier has not published an exact value for DURANEX® 7340, the range is derived from published data for comparable 40% glass-reinforced PBT injection-moulding compounds.
| Property | Test method | Hydrolysis-resistant PBT-GF40 | Standard PBT-GF30 | Standard PBT-GF40 |
|---|---|---|---|---|
| Density | ISO 1183-1 | 1.63–1.69 g/cm³ | 1.52–1.58 g/cm³ | 1.61–1.67 g/cm³ |
| Tensile modulus | ISO 527-2 | 12,000–14,500 MPa | 9,500–11,000 MPa | 11,000–13,500 MPa |
| Tensile stress at break | ISO 527-2 | 120–140 MPa | 100–115 MPa | 115–135 MPa |
| Flexural modulus | ISO 178 | 11,000–13,000 MPa | 8,000–10,000 MPa | 10,000–12,000 MPa |
| Charpy notched impact, 23 °C | ISO 179-1/1eA | 8–11 kJ/m² | 6–9 kJ/m² | 7–10 kJ/m² |
| Heat deflection temperature, 1.8 MPa | ISO 75-1/-2 | 205–215 °C | 200–210 °C | 205–215 °C |
| Water absorption, 24 h immersion | ISO 62 | 0.10–0.20% | 0.15–0.25% | 0.10–0.20% |
These dry values do not rank hydrolytic durability. A hydrolysis-resistant grade may display similar or slightly lower as-moulded tensile strength than a standard grade because the stabilizer package can influence interfacial adhesion. The decisive measurement is retention after pressurised ageing, expressed as a percentage of the original tensile stress at break. For hydrolysis-stabilized PBT-GF40, retention of 70–85% after 500 h at 120 °C in 50:50 water–ethylene glycol is a representative screening target; standard PBT-GF40 can fall below 50% under the same conditions. The test uses sealed pressure vessels with enough liquid to cover the specimens, and the cooling fluid should be sampled for pH shifts because acidic coolant below pH 6.0 accelerates chain scission.
Compared with PA66-GF35 in automotive coolant circuits, PBT-GF40 absorbs less water and maintains modulus better in humid environments, but it offers lower notched impact strength and lower continuous-use temperature under load. Compared with PPS-GF40, the PBT grade processes at a melt temperature roughly 50–70 °C lower and is less abrasive to barrel and tooling, but its creep modulus above 180 °C is lower and its chemical resistance to strong acids and strong bases is limited. Strongly alkaline solutions and hot concentrated acid should be excluded from service; alkaline hydrolysis attacks ester linkages and can override the stabilizer package. Amine-based heat stabilizers or residual polyamide in the hot runner can catalyse transesterification and should be purged before processing; alkaline mould-release agents above pH 9 can also attack the matrix surface.
The shift from 30% to 40% glass fibre changes melt viscosity and fibre orientation. At shear rates typical of injection moulding—100–1,000 s⁻¹—capillary rheometry according to ISO 11443 shows higher viscosity for 40% glass-filled PBT, which increases injection pressure for the same flow length and wall thickness. The melt temperature should be run at 250–270 °C, and the mould should be held at 80–100 °C to crystallize the sealing surfaces and reduce post-mould shrinkage. A mould temperature below 80 °C can produce a glass-rich skin with lower crystallinity and greater warpage after moisture exposure. A mould temperature above 100 °C usually extends cycle time without proportional improvement in crystallinity because PBT crystallizes rapidly even at moderate mould temperatures.
Mould shrinkage is anisotropic. Published values for glass-filled PBT tested according to ISO 294-4 typically fall between 0.2–0.6% in the flow direction and 0.6–1.1% transverse to flow. At 40% glass loading, the orientation layer occupies a larger fraction of the cross-section, so anisotropy can be greater than in a 30% glass grade. Shrinkage prediction for connector housings with thin ribs should not use a single isotropic value; instead, the mould designer should use flow-direction and transverse shrinkage values from cavity-pressure-controlled plaques. Gate location should keep weld lines away from snap-fit arms and sealing grooves because weld-line tensile strength can be less than 60% of the bulk value even before hydrolysis.
Batch-to-batch viscosity variation also becomes more visible at 40% glass loading. A relative melt-flow variation of ± 5% measured by ISO 1133-1 at 250 °C/2.16 kg can shift filling pressure by 8–12% in an eight-cavity hot-runner tool. Process monitoring should therefore use hydraulic transfer pressure and cushion position as control variables rather than fixed injection velocity alone. On a 20:1–22:1 L/D general-purpose screw with a wear-resistant screw tip and check ring, screw speed should be kept to 80–120 min⁻¹, back pressure to 2–5 MPa, and decompression to 3–6 mm to avoid fibre breakage and sprue drool. For valves and seals with thin flash-prone parting lines, clamp force should be calculated from a cavity pressure of 50–80 MPa; thin-wall parts can exceed 80 MPa locally at the gate.
Direct-gated water pump impellers demonstrate the abrasive wear boundary. Continuous flow of 40% glass-filled PBT across gate inserts, screw tips, and check rings accelerates wear compared with 30% glass compounds. Hardened cold-work tool steel such as DIN 1.2379 or equivalent with surface hardness above 56 HRC is preferred for gate inserts and shut-off faces. On a 20:1 L/D injection screw, check-ring leakage can increase after approximately 50,000 cycles with 40% glass-filled PBT; the resulting shot-size drift reduces holding-pressure effectiveness and can create through-thickness porosity in thick bosses. This is not unique to DURANEX® 7340, but the higher fibre fraction raises the number of abrasive particles in the melt and shortens the interval between screw and check-ring inspections.
Datasheet water absorption at 24 h does not rank hot-coolant durability. The more useful screening method exposes ISO 527-2 type 1A tensile specimens to a pressurised liquid mixture at 120 °C for 500 h. The liquid should be 50:50 water–ethylene glycol with inhibitor packages representative of the target vehicle coolant. After ageing, specimens are redried at 80 °C under vacuum until mass change stabilizes, then tested for tensile stress at break and elongation. Retention of elongation at break is often a more sensitive indicator of hydrolysis than tensile strength, because chain scission reduces strain at failure before the ultimate stress is lost. Hydrolysis-stabilized PBT-GF40 typically retains more than 50% of original elongation after 500 h; a standard PBT-GF40 may become brittle and retain less than 25%.
The presence of ethylene glycol changes water activity and can solvate end-groups, so water-immersion data cannot be directly substituted for coolant ageing. Test coupons should be moulded with fully developed fibre skins, and specimens should be edge-sealed only if the application contains a sealed edge. If the part will be in continuous contact with moving coolant, a flow loop with temperature spikes to 130 °C is more representative than a static autoclave because it combines thermal oxidation and hydrolysis with mechanical stress from pressure pulses. Coupon thickness also influences ranking. At wall thicknesses below 1 mm, diffusion paths are short and surface hydrolysis can dominate; at thicknesses above 3 mm, core moisture uptake is slower, but residual packing stress can create internal cavitation that retains coolant. A single set of 4 mm ISO specimens may therefore not predict behaviour in all wall sections.
| Parameter | Boundary or set-point | Reference standard or equipment basis |
|---|---|---|
| Residual moisture after drying | ≤0.02% | ISO 15512:2019, Karl Fischer titration |
| Drying temperature and time | 120 °C, 4–6 h | Desiccant dryer, dew point -35 °C or lower |
| Melt temperature range | 250–270 °C | Barrel set-points with 20:1–22:1 L/D screw |
| Mould temperature | 80–100 °C | ISO 294-4 dimensional stability plaques |
| Residence time above 270 °C | ≤5 min | ISO 11443 capillary rheometry and barrel residence calculation |
| Hot-runner manifold tolerance | ± 5 °C | Multi-cavity hot-runner manifold thermocouple calibration |
| Holding pressure | 60–100 MPa hydraulic cavity pressure | ISO 294-1 injection-moulding pressure measurement |
| Clamp force estimation | 50–80 MPa cavity pressure | Projected area calculation |
| Screw recovery speed | 80–120 min⁻¹ | 40 mm general-purpose screw |
| Back pressure | 2–5 MPa | Injection-unit hydraulic pressure transducer |
For appliance pump housings exposed to 90 °C water and 0.3 MPa line pressure, the combination of 40% glass fibre and hydrolytic stabilization is specified when creep modulus after wet ageing must remain above 4,000 MPa and when dimensional change must stay below 0.2% after 1,000 h. The trade-off is a narrower processing window, higher abrasive wear than 30% glass PBT, and higher tool maintenance frequency. Published data for this specific configuration is limited; therefore, pilot moulding trials with production tooling should verify shrinkage, weld-line placement, and long-term coolant resistance before full qualification.