| HS Code | 278902 |
| Polymer Base | PBT |
| Reinforcement | Glass fiber |
| Glass Fiber Content Percent | 30 |
| Impact Modification | Tough/impact-modified |
| Density G Cm3 | 1.53 |
| Tensile Strength Mpa | 140 |
| Tensile Elongation Percent | 3.0 |
| Flexural Modulus Mpa | 8500 |
| Flexural Strength Mpa | 210 |
| Charpy Notched Impact Kj M2 | 8 |
| Hdt 1 82 Mpa C | 200 |
| Melting Point C | 225 |
| Water Absorption Percent | 0.07 |
| Mold Shrinkage Flow Percent | 0.3 |
| Mold Shrinkage Crossflow Percent | 0.7 |
| Ul94 Flame Rating | HB |
| Volume Resistivity Ohm Cm | 1E16 |
| Dielectric Strength Kv Mm | 20 |
| Coefficient Linear Thermal Expansion 1e 5 C | 3 |
As an accredited Polyplastics DURANEX® PBT+GF30%-Tough 3300H factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Polyplastics DURANEX® PBT+GF30%-Tough 3300H is supplied in 25 kg moisture-resistant, polyethylene-lined paper bags, palletized and shrink-wrapped for industrial shipment. |
| Container Loading (20′ FCL) | 20′ FCL container loaded with Polyplastics DURANEX® PBT+GF30%-Tough 3300H, packed in 25 kg bags on pallets, secured for export shipment. |
| Shipping | Polyplastics DURANEX® PBT+GF30%-Tough 3300H is shipped as pelletized resin in moisture-barrier bags/containers on pallets. It is generally not regulated as dangerous goods for road, sea, or air. Keep dry, cool, ventilated, and protected from sunlight, moisture, and contamination; follow the SDS. |
| Storage | Store Polyplastics DURANEX® PBT+GF30%-Tough 3300H in a cool, dry, well-ventilated area in original sealed packaging. Protect from direct sunlight, heat, moisture, and humidity. Keep away from strong oxidizers and ignition sources; avoid dust generation. Use grounded handling equipment. Ensure containers remain closed when not in use. Do not store near food or beverages. Follow supplier drying recommendations before processing. |
| Shelf Life | Shelf life is typically two years from manufacture when stored cool, dry, and unopened in original packaging; avoid moisture. |
Competitive Polyplastics DURANEX® PBT+GF30%-Tough 3300H prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Polyplastics DURANEX® PBT+GF30%-Tough 3300H is a 30% glass-fiber-reinforced polybutylene terephthalate compound in which a dispersed high-impact modifier is added to the semicrystalline PBT matrix. The grade designation 3300H identifies the toughness-modified variant of the standard 3300 GF30 series. The glass reinforcement is E-glass fiber with a nominal filament diameter of 10–13 µm and a fiber mass fraction verifiable by ash content according to ISO 3451-1 method A. After injection molding, the mean fiber length is typically 200–400 µm, although published data for this specific configuration is limited. Density is reported as 1.53 g/cm³ by ISO 1183-1. The compound is supplied as cylindrical pellets and requires dry storage in sealed containers at temperatures below 30°C. The polymer matrix retains the characteristic semicrystalline PBT morphology, with a melting temperature near 224°C as measured by ISO 11357-3.
In the standard DURANEX 3300 grade, the 30 wt% glass fiber network increases tensile stress at break and flexural modulus relative to unfilled PBT. The high-impact 3300H formulation introduces a rubbery dispersed phase that reduces stress-transfer efficiency at the fiber-matrix interface. Published comparative datasheets show a notched Charpy impact strength increase from approximately 7 kJ/m² in standard 3300 to 10–11 kJ/m² in 3300H, tested at 23°C according to ISO 179-1/1eA. The same modification lowers tensile stress at break from approximately 135 MPa to 125 MPa under ISO 527-2 and lowers flexural modulus from approximately 9.3 GPa to 8.0 GPa under ISO 178. Heat deflection temperature remains approximately 205°C at 1.8 MPa under ISO 75-2/A because the glass fiber network dominates load-bearing at elevated temperature.
| Property | Test method | DURANEX 3300H | DURANEX 3300 |
|---|---|---|---|
| Density | ISO 1183-1 | 1.53 g/cm³ | 1.53 g/cm³ |
| Tensile stress at break | ISO 527-2 | 125 MPa | 135 MPa |
| Tensile elongation at break | ISO 527-2 | 3.0 % | 2.0 % |
| Flexural modulus | ISO 178 | 8.0 GPa | 9.3 GPa |
| Charpy notched impact strength at 23°C | ISO 179-1/1eA | 10 kJ/m² | 7 kJ/m² |
| Heat deflection temperature at 1.8 MPa | ISO 75-2/A | 205°C | 205°C |
| Mold shrinkage, flow direction | ISO 294-4 | 0.3–0.6 % | 0.2–0.5 % |
The trade-off in mechanical properties is not linear with modifier content. At low modifier concentrations, the notched impact strength rises slowly while the flexural modulus decreases; beyond a critical volume fraction, the rubbery phase forms a co-continuous morphology and the modulus drops more sharply. For this reason, 3300H is specified when the governing failure mode is brittle crack propagation at fiber tips, not when maximum static stiffness is required. A standard 3300 grade should be used for structural brackets where deflection must be minimized; 3300H is used for snap-fit hinges, latch arms, and screw bosses that must absorb insertion forces without cracking. The difference in tensile elongation at break—approximately 3.0% for 3300H versus 2.0% for standard 3300 under ISO 527-2—reflects the improved ductility of the matrix.
Microstructurally, the glass fibers act as heterogeneous nucleation sites for PBT crystallization. Differential scanning calorimetry on similar 30% glass-filled PBT compounds shows a crystallization peak temperature near 190–200°C during cooling at 10 K/min under ISO 11357-7. The presence of the impact modifier may shift this peak by several degrees. The resulting transcrystalline layer at the fiber surface improves interfacial shear strength but restricts bulk matrix ductility. In the toughened grade, the modifier forms discrete domains that absorb energy through cavitation and shear yielding. Under notched impact conditions, this phase blunts crack fronts and delays catastrophic fiber pull-out. The mean fiber length after injection molding is therefore an important quality-control parameter; excessive screw recovery speed or high back pressure can reduce fiber length below the critical transfer length and erase the toughness benefit.
Mold shrinkage is anisotropic due to fiber orientation. In flow direction, 3300H typical shrinkage is 0.3–0.6%; transverse shrinkage is 0.6–1.0% according to ISO 294-4. This anisotropy causes warpage in flat parts. The toughness modifier may slightly increase shrinkage compared with standard 3300. Mold-flow simulation with measured shrinkage coefficients and fiber orientation tensors should be used for flat parts with length-to-width ratio above 3:1. When converting from standard 3300, the packing profile should be re-optimized because the higher low-shear viscosity of 3300H changes gate-seal time.
Because the junction of two melt fronts creates fiber orientation largely parallel to the weld line, weld lines are zones of reduced property in glass-filled PBT. The high-impact formulation improves weld-line elongation relative to standard 3300, but weld-line tensile strength remains lower than the base material. The toughness modifier cannot fully compensate for this orientation effect. Gate location should be arranged to move weld lines away from high-tensile regions, and mold-flow simulation should be used to predict weld-line placement.
Before melt processing, the hygroscopic nature of PBT requires closed-loop dehumidified-air drying at 120°C for 4–6 h. The dew point of the drying air should be -30°C or lower, and residual pellet moisture should be ≤0.02 wt% by Karl Fischer titration. In plants where ambient relative humidity exceeds 60% RH, moisture regain is rapid. Molded parts show splay, silver streaks, and reduced notched impact strength when pellet moisture exceeds 0.03 wt% at the hopper. Because the toughness modifier can undergo hydrolytic chain scission at melt temperature, drying is not a cosmetic recommendation but a condition for retaining molecular weight.
On production-scale reciprocating-screw injection molding machines, the melt temperature for DURANEX 3300H is typically set between 240°C and 270°C. A representative barrel profile is rear 240°C, center 250°C, front 260°C, nozzle 265°C. The thermal stability window is narrow; melt temperature above 280°C or total residence time above 10 min produces brown discoloration and measurable loss of notched impact strength. Holding pressure from 40–70 MPa is used to pack out the fiber-filled melt, and back pressure from 0.5–2.0 MPa improves fiber dispersion without excessive shear heating. Screw rotation speed is typically 100–200 rpm on machines with screw diameters of 40–80 mm.
Injection molds for 3300H are maintained at 60–100°C. A mold surface temperature of 80°C is preferred for high-impact applications because slower cooling increases PBT crystallinity and improves notched Charpy impact strength. Below 60°C, molded parts may show reduced impact strength, poor weld-line strength, and gloss variation. The 30% glass-fiber content is abrasive; processors specify bimetallic barrels, hardened check rings, and hardened screw tips. General-purpose screws with L/D 20:1 and compression ratio 2.5:1 are commonly used. Hot-runner systems should have externally heated manifolds with minimum channel diameter 6 mm and no dead spots, because stagnant melt degrades and generates black specks. Cold-runner gates should avoid sharp edges that cause fiber orientation discontinuities and weak weld lines.
Rheological data for 30% glass-filled PBT compounds indicate pseudoplastic flow. At 260°C and a shear rate of 1000 s⁻¹, capillary rheometry shows an apparent melt viscosity in the range of 100–200 Pa·s for similar formulations; the toughener increases low-shear viscosity relative to standard 3300. This higher viscosity reduces flash in precision molds but increases pressure drop in long flow paths. Spiral flow at 2 mm wall thickness is shorter than for unfilled PBT; wall thickness below 1.5 mm should be analyzed with mold-flow simulation using measured viscosity data. Gate freeze time is reduced by glass fibers; gate diameter should be at least 0.8–1.0 mm for larger parts, and the gate land length should be minimized to prevent premature freeze-off.
On the manufacturing floor, lot-to-lot variation is monitored by melt volume-flow rate and notched Charpy impact tests on conditioned plaques. Conditioning at 23°C and 50% RH for 48 h under ISO 291 is required before impact testing because PBT absorbs moisture and the notched impact value shifts with water content. Tensile test specimens are prepared to ISO 527-2 type 1A; flexural specimens to ISO 178. The glass fiber content is checked by ash content ISO 3451-1; ash values outside the control range indicate either let-down error or screw wear contamination.
Snap-fit hinges, latch arms, and screw bosses in automotive electrical connectors are typical applications for 3300H because the standard 3300 grade may fracture during assembly. The notched Charpy impact strength of 10–11 kJ/m² at 23°C allows deflection-dependent features to absorb insertion forces without cracking. In power tool housings, the glass-fiber network controls creep under clamp load, while the toughener prevents brittle failure at rib roots and vent openings. In relay bases and terminal blocks, the grade provides dimensional stability under electrical heating and resistance to fracture during wiring assembly. For components that must survive drop testing, the high-impact formulation is used instead of standard 3300 when the drop test protocol requires no crack initiation from a specified height.
Continuous service in air above 100°C should be validated by thermal aging at the specific wall thickness. Resistance to hot water and automotive antifreeze is limited; PBT hydrolyzes in hot-wet environments above 80°C, and the impact modifier may accelerate this embrittlement. For coolant-contacting parts, a hydrolysis-resistant DURANEX grade should be selected. The material is not a flame-retardant grade; applications requiring UL 94 V-0 at 0.75 mm require a flame-retarded DURANEX series. Outdoor weathering also requires UV stabilization unless the part is painted or shielded; published data for this specific configuration is limited. Avoid use with strong alkaline solutions, amines, or hot organic solvents because PBT undergoes ester hydrolysis and environmental stress cracking.
Compliance documentation for 3300H is grade-specific and should be requested from Polyplastics for the production site. The compound is typically certified to RoHS Directive 2011/65/EU and REACH Regulation (EC) No 1907/2006. UL recognition is often listed as UL 94 HB at 0.75 mm, but the yellow card must be confirmed for the actual color and thickness. Lot certificates provide density, melt volume-flow rate, tensile stress at break, elongation at break, flexural modulus, and notched Charpy impact strength under the relevant ISO methods. The ISO 11469 marking for molded parts is >PBT+GF30<; the recycling code is 07. For food-contact or medical applications, published data for this specific configuration is limited; FDA 21 CFR 177.1660 or ISO 10993 testing is outside the standard grade certification and must be performed on the final article.