| HS Code | 699420 |
| Polymer Type | PBT |
| Reinforcement | 30% glass fiber |
| Density | 1.53 g/cm³ |
| Water Absorption 24 H | 0.07% |
| Tensile Strength | 140 MPa |
| Elongation At Break | 2.5% |
| Flexural Modulus | 9,000 MPa |
| Charpy Notched Impact Strength 23 C | 9 kJ/m² |
| Heat Deflection Temperature 1 82 Mpa | 205°C |
| Melting Point | 224°C |
| Mold Shrinkage Flow Direction | 0.2–0.5% |
| Ul Flammability Rating | HB |
| Volume Resistivity | 1×10^16 Ω·cm |
| Dielectric Strength | 20 kV/mm |
| Recommended Melt Temperature | 250–270°C |
| Drying Conditions | 120°C for 3–4 h |
As an accredited Polyplastics DURANEX® PBT+GF30%-High-Temp 7500 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Polyplastics DURANEX® PBT+GF30%-High-Temp 7500 supplied in 25 kg moisture-barrier bags, palletized and clearly labeled with grade and lot details. |
| Container Loading (20′ FCL) | 20′ FCL container loaded with Polyplastics DURANEX® PBT+GF30%-High-Temp 7500, securely palletized, stowed in dry conditions, and sealed for export shipment. |
| Shipping | DURANEX® PBT+GF30%-High-Temp 7500 is supplied as non-hazardous thermoplastic pellets in sealed moisture-barrier bags or boxes. Ship in cool, dry conditions; avoid direct sunlight, moisture, and high temperatures. Keep containers closed, label appropriately, and follow the SDS and local regulations. No special DG declaration is typically required unless specified. |
| Storage | Store DURANEX PBT+GF30%-High-Temp 7500 in a cool, dry, well-ventilated area, away from direct sunlight, heat, ignition sources, and incompatible chemicals. Keep containers sealed, labeled, and in original packaging to prevent moisture absorption and contamination. Avoid prolonged UV/humidity exposure; use first-in, first-out. Maintain stable ambient temperature and follow local regulations and SDS recommendations. Store separately from acids, bases, oxidizers, and solvents. |
| Shelf Life | Shelf life: 12 months from date of manufacture when stored unopened in a dry, cool place, protected from sunlight. |
Competitive Polyplastics DURANEX® PBT+GF30%-High-Temp 7500 prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Polyplastics DURANEX® PBT+GF30%-High-Temp 7500 is a heat-stabilized 30 wt% glass-fibre reinforced polybutylene terephthalate injection-moulding compound. The grade is identified by the model designation 7500 and is supplied as cylindrical pellets. The material is specified for components in which dimensional stability, flexural stiffness, and electrical insulation must be retained after prolonged exposure to elevated ambient temperatures. Under ISO 1183-1, density falls within a representative range of 1.54–1.56 g/cm³. Melt volume-flow rate measured under ISO 1133-1 at 250°C and 2.16 kg is typically reported between 12 cm³/10 min and 20 cm³/10 min. Tensile stress at break under ISO 527-1/-2 is in the range of 130–140 MPa for a 5A specimen after conditioning at 23°C and 50% relative humidity per ISO 291. Flexural modulus under ISO 178 is in the range of 8200–9000 MPa. These values are representative of the heat-stabilized 30% glass-fibre PBT material class and should be verified against the current lot certificate because minor shifts arise from colorant and additive packages.
| Property | Test method | Heat-stabilized 7500 grade | Standard GF30 PBT |
| Density | ISO 1183-1 | 1.54–1.56 g/cm³ | 1.52–1.54 g/cm³ |
| Tensile stress at break | ISO 527-1/-2 | 130–140 MPa | 120–135 MPa |
| Flexural modulus | ISO 178 | 8200–9000 MPa | 8000–8500 MPa |
| Heat deflection temperature, 1.8 MPa | ISO 75-1/-2 | 200–210°C | 195–205°C |
| Melt volume-flow rate | ISO 1133-1 | 12–20 cm³/10 min | 8–16 cm³/10 min |
| Comparative tracking index | IEC 60112 | 500–600 V | 250–350 V |
Oxidative degradation in polybutylene terephthalate proceeds through radical-mediated chain scission at the ester linkages. The heat-stabilization system in the 7500 grade functions as a free-radical scavenger and hydroperoxide decomposer, delaying the autocatalytic oxidation cycle that causes surface embrittlement and loss of tensile elongation. Retention of tensile strength after thermal exposure is evaluated under ISO 527-1/-2 after oven aging at temperatures from 150°C to 180°C. Time-to-50% tensile strength loss is commonly used as an acceptance criterion in component qualification. Components moulded from the heat-stabilized grade are typically considered for continuous-use temperatures up to 130°C, with short-term excursions to 180°C permissible only when electrical load, part wall thickness, and airflow have been verified. UL 746B relative thermal index values for specific colors and thicknesses provide regulatory confirmation of long-term thermal capability, but the exact listing for this grade and color must be checked because published data for this specific configuration is limited.
For continuous underhood service, the material is used in charge-air temperature sensor frames, camshaft position sensor housings, and connector bodies mounted directly to the cylinder head cover. The heat-stabilized formulation reduces the surface embrittlement observed in standard GF30 PBT after repeated thermal cycling from -40°C to 150°C. In e-mobility applications, the compound appears in high-voltage interlock connector housings and battery management system insulation plates, where dimensional stability under mechanical load is evaluated through ISO 75-1/-2 heat deflection temperature. The 30 wt% glass reinforcement raises the flexural modulus to a representative range of 8200–9000 MPa under ISO 178, compared with approximately 2500–2800 MPa for unfilled polybutylene terephthalate. This stiffness increase allows reduced wall thickness in connector shells without exceeding the allowable deflection at service temperature.
The melt is processed with cylinder nozzle settings of 250°C to 270°C; the barrel profile from rear zone to metering zone typically rises from 240°C to 265°C. Pre-drying in a desiccant dryer at 120°C for 4–6 hours is required when the initial moisture content exceeds 0.02 wt%. Because hydrolysis reduces molecular weight at processing temperatures, hopper residence time after drying should not exceed 30 minutes unless a dry-air blanket is maintained. The compound is injection-moulded with screw L/D ratios of 20:1 to 25:1 and compression ratios of 2.5:1 to 3.0:1. High-shear screw designs with narrow mixing clearances may generate excessive frictional heat and should be avoided. General-purpose polyolefin screws are commonly used; long glass-fibre screws are not required for this short-glass product. Shot size should occupy 30–70% of barrel capacity to limit residence time and thermal history.
Mold temperature is maintained between 80°C and 100°C to promote full crystallization and to minimize post-mould shrinkage. At wall thickness below 1.0 mm, injection velocity must be increased, but melt residence time should remain below 5 minutes to prevent thermal degradation and the formation of black specks in the final part. Hydraulic injection pressure in production equipment typically falls between 70 MPa and 120 MPa, with hold pressure set at 50–70% of the peak injection pressure. Clamp force requirements for glass-filled polyester compounds are commonly estimated at 3–5 kN/cm² of projected moulded area. Insufficient clamp force produces flash at the parting line because the low melt viscosity at 260°C permits penetration into clearances as small as 0.01 mm. Published data for this specific configuration for all machine and tool combinations is limited, so process capability trials on the intended mould are required.
Because the 30 wt% glass-fibre reinforcement creates anisotropic shrinkage, part designs with abrupt wall-thickness transitions are prone to differential cooling and internal stress. Gate location should place high shear zones away from areas that carry mechanical load, particularly adjacent to metal insert edges. Weld-line strength in glass-filled PBT typically retains only 40–60% of the unfilled matrix strength; this is a limiting factor in complex connector housings with multiple pin holes. Post-mould annealing at 150°C for 2 hours may be applied to relieve moulded-in stress, but only after dimensional fixtures have been used to prevent warpage. These operational boundaries distinguish the 7500 grade from unreinforced DURANEX 2002, which exhibits lower modulus and lower shrinkage anisotropy but cannot sustain creep loads above 90°C without excessive deformation.
Substitution of standard 30% glass-fibre PBT with the heat-stabilized 7500 grade is justified where comparative tracking index performance under IEC 60112 is an acceptance criterion. Where the standard grade may exhibit tracking index values in the 250–350 V range, the 7500 series is formulated to achieve higher resistance, frequently reaching 500–600 V under test condition A. This difference is relevant for printed-circuit-board connectors with creepage distances below 4.0 mm at operating voltages above 400 V. The heat-stabilization package also extends the retention of dielectric strength after thermal cycling, as measured by IEC 60243-1. However, the grade is not inherently flame-retarded; where UL 94 V-0 at 0.75 mm is required, the design should evaluate DURANEX 6300B or an equivalent flame-retarded PBT instead of the 7500 grade. This distinction is critical because heat stabilization and flame retardancy are separate additive packages that influence melt viscosity, plating adhesion, and color stability differently.
| Requirement | Test method or standard | Typical condition |
| Tensile properties | ISO 527-1/-2 | 5A specimen, 1 mm/min, conditioned at 23°C/50% RH |
| Flexural properties | ISO 178 | 80×10×4 mm specimen, 2 mm/min |
| Heat deflection temperature | ISO 75-1/-2 | 1.8 MPa, flatwise |
| Melt volume-flow rate | ISO 1133-1 | 250°C/2.16 kg |
| Comparative tracking index | IEC 60112 | Solution A, 100 drops |
| Dielectric strength | IEC 60243-1 | 1 mm disc in transformer oil |
| Oven aging | ISO 527-1/-2 after aging | 150–180°C, forced-air oven |
| Relative thermal index | UL 746B | Color- and thickness-specific listing required |
For sealed power electronics housings exposed to high humidity, the hydrolytic stability of PBT remains a boundary condition. Long-term exposure to water-glycol mixtures above 60°C or continuous operation in 85% relative humidity at 85°C can reduce tensile strength through ester bond hydrolysis. The 7500 grade is not recommended for use in direct contact with engine coolant, strong acids, or steam-autoclave sterilization cycles above 121°C. Compatibility with automotive oils, greases, and unleaded fuels is generally acceptable at ambient temperatures, but immersion testing per ISO 175 should be conducted for any new fluid formulation. Ultraviolet exposure should be considered only when the component is enclosed because PBT-GF30 surfaces may develop chalking and a reduction in impact resistance after outdoor weathering. Published data for this specific configuration under accelerated weathering is limited; therefore, unpainted exterior applications require validation under ISO 4892-2 or ISO 4892-3.