Polyplastics Duranex Pbt Gf30 Fr Nf 330nf

Polyplastics DURANEX® PBT+GF30%-FR-NF 330NF

    • Product Name: Polyplastics DURANEX® PBT+GF30%-FR-NF 330NF
    • Factroy Site: Yinchuan, Ningxia, China
    • Price Inquiry: sales8@ascent-chem.com
    • Manufacturer: Ascent Petrochem Holdings Co., Limited
    • CONTACT NOW
    VTB
    Specifications
    HS Code 833410
    Density 1.60 g/cm³
    Glass Fiber Content 30%
    Flame Retardancy UL94 V-0
    Tensile Strength 125 MPa
    Tensile Elongation At Break 2.0%
    Flexural Modulus 9,000 MPa
    Flexural Strength 180 MPa
    Charpy Notched Impact Strength 8 kJ/m²
    Heat Deflection Temperature At 1 8 Mpa 200 °C
    Melting Point 225 °C
    Molding Shrinkage In Flow Direction 0.3%
    Molding Shrinkage In Cross Flow Direction 0.8%
    Water Absorption At 23 C 24 H 0.2%
    Volume Resistivity 1×10^16 Ω·cm
    Dielectric Strength 20 kV/mm
    Comparative Tracking Index 600 V

    As an accredited Polyplastics DURANEX® PBT+GF30%-FR-NF 330NF factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.

    Packing & Storage
    Packing Polyplastics DURANEX® PBT+GF30%-FR-NF 330NF is supplied in 25 kg sealed moisture-barrier bags, 40 bags (1,000 kg) per pallet.
    Container Loading (20′ FCL) 20′ FCL container loaded with palletized 25 kg bags of Polyplastics DURANEX® PBT+GF30%-FR-NF 330NF, secured for ocean shipment.
    Shipping Polyplastics DURANEX® PBT+GF30%-FR-NF 330NF is shipped as non-hazardous, moisture-sensitive thermoplastic pellets in sealed foil-lined bags, fiber drums, or bulk containers. Keep dry, cool, and away from direct sunlight; avoid moisture uptake and high temperatures. Refer to SDS and local regulations for handling and transport.
    Storage Store DURANEX® PBT+GF30%-FR-NF 330NF in a cool, dry, well-ventilated area away from direct sunlight, heat sources, and ignition. Keep containers closed to prevent moisture pickup and contamination. Avoid dust generation and static buildup; use grounding where applicable. Segregate from strong oxidizers, acids, and bases. Protect packaging from physical damage and follow local regulations and the manufacturer’s safety data sheet.
    Shelf Life Typical shelf life is 24 months when stored dry, cool, and in original sealed packaging, protected from moisture and sunlight.
    Free Quote

    Competitive Polyplastics DURANEX® PBT+GF30%-FR-NF 330NF prices that fit your budget—flexible terms and customized quotes for every order.

    For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.

    We will respond to you as soon as possible.

    Tel: +8618005193850

    Email: sales8@ascent-chem.com

    Inquiry

    Get Free Quote of Ascent Petrochem Holdings Co., Limited

    Flexible payment, competitive price, premium service - Inquire now!

    Certification & Compliance
    More Introduction

    Polyplastics DURANEX® PBT+GF30%-FR-NF 330NF is a 30 wt% glass-fiber-reinforced polybutylene terephthalate compound supplied under the DURANEX FR-NF flame-retardant designation. The model designation identifies the core formulation segment: PBT matrix, 30% short-glass reinforcement, and a flame-retardant package classified within the supplier’s FR-NF series. The grade is intended for injection-molded electrical and electronic components requiring thin-wall flame retardance, high rigidity, low mold shrinkage, and dimensional stability under elevated service temperatures. The suffix coding is supplier-specific; FR-NF does not by itself establish a food-contact or non-food-contact status, and the lot certificate should be consulted before release for food-adjacent or safety-critical service.

    Glass content is verified by thermogravimetric ash analysis in accordance with ISO 3451-1. In the compounded pellet, the glass fiber length distribution after injection molding is typically shorter than the original chopped strand length. Post-compounding number-average fiber lengths in the range of 200–400 µm are representative of side-fed glass incorporation on a co-rotating twin-screw line. Retention of the fiber length determines the tensile modulus and notched impact stability. Because the matrix is semi-crystalline polybutylene terephthalate with an ester backbone, the material is moisture-sensitive during processing and requires controlled pre-drying.

    Density of 30% glass-fiber flame-retardant PBT grades is typically 1.62–1.67 g/cm³ when measured by ISO 1183-1. Tensile modulus under ISO 527-1/-2 at 23°C is typically in the range 9,000–10,500 MPa. Heat deflection temperature under 1.8 MPa load by ISO 75-1/-2 is typically 195–210°C. Mold shrinkage in the flow direction measured by ISO 294-4 is typically 0.2–0.6%. These are representative industrial ranges for 30% glass-filled flame-retardant PBT and are not a substitute for lot-specific certificate-of-analysis values for 330NF.

    The primary usage envelope is injection-molded connectors, relay housings, terminal blocks, coil bobbins, sensor bodies, and breaker secondary covers. The combination of UL 94 V-0 flame retardance at 0.8 mm thickness and 30% glass reinforcement reduces creep and improves dimensional stability compared with unfilled PBT. This renders the material suitable for components that locate contacts and maintain creepage and clearance distances under thermal load.

    Compared with unfilled PBT, the 30% glass-reinforced flame-retardant grade increases tensile modulus by approximately 3-fold and reduces flow-direction mold shrinkage by roughly 70%. Compared with 30% glass-filled PBT that is not flame retardant, the flame-retardant package raises density and can reduce notched impact strength by 10–20%. These trade-offs are quantified in the comparative table below.

    What Limits the Injection Molding Window for 330NF at 30% Glass Loading?

    Pre-drying at 120°C in a desiccant hopper dryer for 4–6 h is required to reduce residual moisture below 0.02%. PBT hydrolyzes at melt temperature when moisture is present; the result is molecular weight reduction, splay on part surfaces, and lower elongation at break. On a production line, a 1,000 kg container left open at 60% relative humidity for more than 8 h typically requires re-drying before molding. Moisture levels above 0.05% are considered unacceptable for thin-wall connector molding because surface defects and property loss occur before visible splay appears.

    The melt temperature measured by an immersion probe should be held between 250°C and 270°C. Above 280°C at residence times exceeding 5 min, the flame-retardant package can decompose and produce plate-out on mold surfaces, black specks, and corrosive by-products. A flat or reverse barrel profile from rear 240°C to front 260°C is commonly used. Screw back pressure between 0.5 MPa and 1.0 MPa densifies the glass-filled melt without excessive shear heating. The practical processing window is narrow because melt temperature below 250°C can raise viscosity sufficiently to limit thin-wall fill, while temperatures above 270°C accelerate degradation. This 20°C melt window places emphasis on shot-size utilization; when shot mass is less than 25% of barrel capacity, residence time increases and degradation by-products may accelerate deposit formation.

    Injection velocity should be profiled to keep gate shear rates below 1,000 s⁻¹. Excessive shear causes local fiber breakage and reduces weld-line strength. In multi-pin connector housings, weld lines form behind each core pin; their tensile strength may be only 50–60% of the bulk value because glass fibers orient parallel to the flow front. Increasing melt temperature within the allowed window can improve weld-line toughness but increases cycle time and degradation risk.

    Mold temperature should be set between 80°C and 100°C. At mold temperatures below 60°C, the outer surface freezes before full crystallization, producing anisotropic shrinkage and post-mold warpage in thin sections. At mold temperatures above 120°C, cycle time increases without proportional gain in crystallinity. For parts with wall thickness below 1.0 mm, high mold temperature is more critical because short-shot limits may force higher melt temperatures. A processing conflict exists between improving weld-line strength at higher melt temperature and restricting flame-retardant decomposition; mold-filling simulation should therefore be used before steel cutting.

    Melt Filtration and Screw Design in GF30 FR PBT Compounding

    Compounding of 30% glass-filled flame-retardant PBT is performed on co-rotating twin-screw extruders with L/D 40:1 or 44:1. The base PBT and flame-retardant masterbatch are fed at the main feed throat, while glass fiber is side-fed after the melting zone to limit fiber attrition. Screw configurations use high-free-volume elements at the fiber feed port, followed by mild kneading and vacuum devolatilization at -0.08 MPa to remove residual moisture and low-molecular-weight volatiles.

    Melt filtration through 80/120 mesh screen packs removes agglomerated flame-retardant particles and fiber bundles. A sustained pressure drop above 10 MPa across the screen indicates filter loading or fiber compaction. Production-scale screw and barrel linings are nitride-hardened or bimetallic because the glass reinforcement accelerates wear; maintenance intervals for screw inspection are generally shorter than for unfilled PBT. Pellet dusting equipment is used before packaging to remove fine glass dust from pellet surfaces, which otherwise enters the hopper and causes feed-bridge or nozzle clogging.

    When Hot-Runner Tooling Is Selected for FR-PBT Connector Housings

    Valve-gated hot-runner systems with independently controlled tip temperatures are preferred over open-gate systems for flame-retardant PBT. The melt should not remain static in the manifold above 280°C. Thermal gradients across a 16-cavity manifold should be held below 3°C to avoid asymmetric gate freeze-off and cavity-to-cavity weight variation.

    Gate land shear rates should be kept below 1,000 s⁻¹. Hot-runner tips should be polished and free of dead spots because flame-retardant additives can deposit on rough surfaces and generate black specks. If stringing or gate blush occurs, tip temperature should be reduced in 5°C increments before valve timing is adjusted. For connector housings with wall thickness 0.8–2.0 mm, nozzle tip orifices of 0.8–2.0 mm are typical. The runner system should be designed with balanced natural or symmetrically split runners; unbalanced runner layouts in glass-filled PBT amplify fiber-orientation driven warpage.

    The Flammability Package Introduces Measured Property Trade-Offs

    The table below presents representative property ranges for unfilled PBT, 30% glass-filled non-flame-retardant PBT, and the 330NF class of flame-retardant 30% glass-filled PBT. Values are typical industrial ranges from standards-conforming test methods, not specification limits for any individual lot.

    Property / Method Unfilled PBT GF30 PBT non-FR 330NF class
    Density, ISO 1183-1 1.30–1.32 g/cm³ 1.50–1.53 g/cm³ 1.62–1.67 g/cm³
    Tensile modulus, ISO 527-1/-2 2,500–2,900 MPa 8,800–10,000 MPa 9,000–10,500 MPa
    HDT/A at 1.8 MPa, ISO 75-1/-2 55–65°C 200–210°C 195–210°C
    Mold shrinkage parallel, ISO 294-4 1.8–2.2% 0.3–0.6% 0.2–0.6%
    Flammability at 0.8 mm, UL 94 V HB HB V-0

    The observed differences arise from two independent modifications: the 30% glass reinforcement and the flame-retardant package. Glass fibers increase tensile modulus, reduce mold shrinkage, and raise heat deflection temperature under load. The flame-retardant package introduces additional filler or reactive species that increase density, may reduce Charpy notched impact strength, and alter tracking performance under IEC 60112.

    For parts that require both UL 94 V-0 and high tracking resistance, the comparative tracking index must be verified. Published data for this specific configuration is limited; CTI for glass-filled flame-retardant PBT can range from 200 V to 600 V depending on flame-retardant chemistry and filler package. The voltage used in creepage distance calculations per IEC 60664-1 should therefore be based on supplier lot data, not on generic PBT assumptions. Halogenated systems may suppress CTI relative to halogen-free systems; no universal FR-NF chemistry should be assumed for 330NF.

    Compliance, thermal aging, and electrical-test standards applicable to molded parts produced from 330NF include the following matrix. The test condition is the primary screening condition because performance at final part thickness may differ from laboratory specimen results.

    Standard Condition Application relevance
    UL 94 V 0.8 mm vertical burn Enclosure flammability classification for unattended electrical parts
    IEC 60112 250 V / 0.1% ammonium chloride Tracking index used for creepage distance calculation per IEC 60664-1
    IEC 60695-2-11 750°C glow wire Glow-wire flammability for appliance components
    IEC 60243-1 1.0 mm thickness, 50 Hz Dielectric strength for connector insulation
    ISO 527-1/-2 23°C, 5 mm/min Tensile modulus and tensile strength
    ISO 179-1/1eA 23°C, notched Charpy notched impact sensitivity

    For application release, part geometry and final wall thickness are more important than pellet-level test results. A UL 94 V-0 pellet classification at 0.8 mm does not automatically confer V-0 on parts with ribs, bosses, or weld lines at the same nominal thickness. Similarly, CTI values obtained on 3.0 mm plaques under IEC 60112 may not apply directly to thin-wall connector walls.

    Production-scale applications for DURANEX® PBT+GF30%-FR-NF 330NF are concentrated in electrical and electronic housings, relay bases, terminal strips, sensor and actuator bodies, and structural frames inside office automation equipment. The material is specified where dimensional stability under heat and humidity, stiffness, and defined flammability rating are simultaneous requirements. Low moisture absorption relative to polyamides supports stable electrical clearances in humid environments; however, PBT is not a substitute for high-temperature polymers such as PPS or LCP where continuous-use temperatures exceed 140°C under load.

    Operational boundaries require attention to hydrolysis and regrind. The material should not be combined with strongly alkaline media, primary amines, or metal soaps that catalyze ester hydrolysis. Regrind addition above 20% accelerates glass-fiber length reduction and can shift mechanical properties outside part drawing limits. Storage should be in sealed containers below 30°C and below 60% relative humidity. After moisture exposure, re-drying at 120°C for 4 h is mandatory before molding.

    Differences from other products in the DURANEX PBT range include the combination of 30% glass reinforcement and the FR-NF flame-retardant package. Unfilled grades process at lower viscosity and exhibit higher shrinkage; non-flame-retardant 30% glass grades may exhibit higher notched impact and lower density but do not provide UL 94 V-0. Halogen-free FR alternatives may be selected for low-smoke or low-corrosivity applications but can introduce different flow and tracking trade-offs. Published data for this specific 330NF configuration is limited for comparative tracking index and glow-wire ignition temperature; final application approval should use lot-specific certificates and part testing.

    Top