| HS Code | 410356 |
| Product | Polyplastics DURANEX® Hydrolytic PBT 201HR |
| Polymertype | Polybutylene terephthalate (PBT) |
| Fillerreinforcement | Unfilled |
| Hydrolysisresistance | Hydrolysis-resistant grade |
| Density | 1.31 g/cm³ |
| Moldshrinkage | 1.5–2.0% |
| Waterabsorption24h | 0.20% |
| Tensilestrength | 55 MPa |
| Elongationatbreak | 30% |
| Flexuralmodulus | 2500 MPa |
| Flexuralstrength | 85 MPa |
| Charpynotchedimpactstrength23c | 3.0 kJ/m² |
| Hdt0 45mpa | 150 °C |
| Hdt1 82mpa | 60 °C |
| Meltingtemperature | 224 °C |
| Ul94flammability | HB |
| Volumeresistivity | 1×10^16 Ω·cm |
| Dielectricstrength | 20 kV/mm |
As an accredited Polyplastics DURANEX® Hydrolytic PBT 201HR factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | DURANEX® Hydrolytic PBT 201HR is typically supplied in 25 kg moisture-barrier bags, palletized at 1,000 kg per pallet. |
| Container Loading (20′ FCL) | 20′ FCL: Polyplastics DURANEX® Hydrolytic PBT 201HR loaded in original sealed packaging, palletized, evenly distributed, and secured for ocean transport. |
| Shipping | Polyplastics DURANEX® Hydrolytic PBT 201HR is a non-hazardous polybutylene terephthalate resin shipped in sealed, moisture-barrier bags or containers. Store and transport in a dry, cool, ventilated area away from direct sunlight, heat, and moisture. No special dangerous-goods classification is expected; verify current SDS and local regulations. |
| Storage | Store DURANEX® Hydrolytic PBT 201HR in a cool, dry, well-ventilated area away from direct sunlight, heat, ignition sources, and oxidizing materials. Keep containers tightly closed to prevent moisture pickup and contamination. Avoid humid conditions and follow first-in, first-out stock rotation. Before processing, dry the resin according to the manufacturer’s recommendations to maintain hydrolytic stability. |
| Shelf Life | Polyplastics DURANEX® Hydrolytic PBT 201HR typically has a 12-month shelf life when stored dry, cool, and in original unopened packaging. |
Competitive Polyplastics DURANEX® Hydrolytic PBT 201HR prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Polyplastics DURANEX® Hydrolytic PBT 201HR is an injection-moulding grade of polybutylene terephthalate engineered for hot-moisture service. The product belongs to the hydrolysis-resistant segment of the DURANEX PBT family and is specified where conventional PBT grades lose tensile elongation and impact strength after prolonged damp-heat exposure. Typical part categories include automotive wiring connectors, sensor housings, relay sockets, and underhood electrical enclosures. The grade is not a fibre-reinforced compound; its technical profile points to an unfilled hydrolytically stabilised base resin. Because PBT crystallises rapidly as a semi-crystalline polyester, the material retains the general solvent resistance, fast moulding cycles, and low equilibrium moisture uptake of PBT, while the stabiliser system differentiates it from general-purpose PBT in autoclave and damp-heat evaluations. Material-property determinations for this resin class are conventionally conducted according to ISO 527-1/-2 for tensile behaviour, ISO 179-1/1eA for Charpy impact, ISO 75-1/-2 for deflection temperature, and ISO 1133-1 for melt volume-flow rate. Published datasheet values for the exact grade-specific retention performance after 85 °C/85 % RH or pressurised hot-water exposure should be confirmed against the current Polyplastics technical datasheet.
The failure mechanism in unmodified PBT is ester linkage hydrolysis followed by chain scission. Water attacks the ester groups along the polybutylene terephthalate backbone, producing carboxylic acid end groups and hydroxyl-terminated fragments. The released acid end groups accelerate further hydrolysis autocatalytically, so the degradation rate is not linear with time; once the acid concentration exceeds a critical threshold, molecular weight declines rapidly. Tensile elongation at break is more sensitive to this chain-length reduction than tensile strength, and parts that appear dimensionally stable may lose ductility before visible cracking occurs. Under automotive qualification conditions such as 85 °C/85 % RH damp heat or 121 °C pressurised steam, standard PBT can pass short-term tests but fail after extended exposure when the molecular-weight distribution shifts toward shorter chains. The practical result is brittle fracture at connector latch features, terminal retention slots, or thin-wall sensor bodies after exposure that would not affect dry as-moulded parts.
Hydrolysis-resistant PBT grades are formulated to suppress the autocatalytic loop rather than merely delay initial moisture absorption. Additive strategies include acid scavenging, chain extension, and end-group capping, all of which reduce the concentration of free carboxylic acid species available to catalyse further ester cleavage. In a grade such as DURANEX 201HR, the stabilisation approach is intended to maintain a higher fraction of original molecular weight after damp-heat ageing when compared with standard unfilled PBT. Because melt viscosity and melt volume-flow rate are functions of average molecular weight, ISO 1133-1:2022 melt-flow measurement before and after ageing is used as a sensitive indicator of chain scission. A large increase in melt volume-flow rate after accelerated ageing would indicate molecular-weight loss, whereas a smaller shift is consistent with hydrolytic stabilisation. Short-term dry mechanical properties are usually similar to those of standard PBT because the stabilisation package primarily affects the ageing trajectory rather than initial stiffness. The material therefore should not be selected solely on the basis of as-moulded tensile strength; specification should include damp-heat property-retention requirements.
Before injection moulding, the moisture content of hydrolytically stabilised PBT should be reduced to below 0.02 % by weight to avoid molecular-weight loss during plastication. Dehumidified air drying at 120 °C for 4 h is a commonly applied PBT drying window, although actual moisture content should be verified by a calibrated moisture analyser. Residual moisture above the target limit can generate surface splay and reduce melt strength, and in hydrolytically sensitive polyester resin the same moisture can contribute to chain scission inside the barrel. Desiccant-bed dryers delivering a dew point of −40 °C or lower are preferred. Drying time must be extended only within the material supplier’s recommended envelope because excessive residence at high temperature can cause thermal yellowing and embrittlement.
The processing window for unfilled hydrolysis-resistant PBT is narrow in comparison with polyolefins and requires control of melt temperature, screw recovery, and mould temperature. Melt temperatures in the range of 240 °C to 270 °C are typical for injection-moulding unfilled PBT, with lower settings used for thin-wall parts and higher settings for longer flow lengths. Mould temperatures between 40 °C and 80 °C govern crystallinity development and shrinkage. If the mould is too cold, the surface freezes before the core develops sufficient crystallinity, producing post-mould warpage and residual stress. In hydrolytically sensitive grades, residual stress is especially relevant because stressed polymer chains are more susceptible to environmental stress cracking when exposed to hot moisture. Gate and runner sizing should therefore be designed to avoid excessive packing pressure decay and uncontrolled shear heating. Screw L/D ratios commonly used for PBT are in the range of 20:1 to 24:1 with a compression zone and a free-flow non-return valve. Published processing documentation for the specific 201HR configuration should be consulted for exact set-points.
Compared with standard unfilled PBT, DURANEX 201HR is selected when damp-heat property retention is part of the part-approval plan. Dry as-moulded tensile strength and flexural modulus are likely to be close to conventional unfilled PBT values, but the product differentiator is the maintenance of elongation and impact after ageing. For example, a standard PBT connector body may retain only a limited fraction of original elongation after 85 °C/85 % RH exposure, whereas a hydrolytically stabilised grade is intended to extend the time to embrittlement. The exact retention improvement depends on part thickness, moulded-in stress, and terminal insertion design. In contrast, a 30 % glass-fibre-reinforced PBT grade offers higher flexural modulus and lower elongation but also displays anisotropic shrinkage and greater notch sensitivity; DURANEX 201HR, as an unfilled type, presents lower stiffness and more isotropic mould shrinkage. Against PBT/PET blends, 201HR is positioned toward improved hydrolytic stability rather than lower-cost blending. For continuous-use temperatures above the PBT practical limit, high-temperature polyamide, PPS, or PPA is normally evaluated instead.
| Test method | Typical exposure or condition | Reported property |
|---|---|---|
| ISO 527-2:2012 | 23 °C, 5 mm/min; aged and unaged specimens | Tensile strength and elongation at break |
| ISO 179-1/1eA:2023 | Notched Charpy, 23 °C; aged specimens | Impact strength after hot-moisture exposure |
| ISO 1133-1:2022 | 250 °C, 2.16 kg | Melt volume-flow rate shift as chain-scission indicator |
| IEC 60068-2-78 | 85 °C, 85 % RH, 1000 h | Damp-heat durability reference |
| ISO 62:2008 | 23 °C, 24 h immersion | Water-absorption baseline |
| ISO 75-2:2013 | 0.45 MPa or 1.8 MPa flexural load | Heat deflection temperature |
| IEC 60112:2020 | Platinum electrode method | Comparative tracking index |
The table represents a qualification framework rather than a substitute for the current Polyplastics datasheet. Reported retention values for DURANEX 201HR after each exposure must be taken from the grade-specific technical datasheet or directly from the supplier. For applications requiring flame retardancy, a separate UL classification applies, and UL 94 performance is thickness-dependent. Hydrolytic stabilisation is not equivalent to flame-retardant modification, and the two requirements should be specified independently. Automotive connector programmes commonly supplement these standards with OEM-specific damp-heat and thermal-shock sequences that include terminal-insertion force testing after ageing.
Application of DURANEX 201HR should be restricted to environments consistent with the thermal and chemical profile of polybutylene terephthalate. Continuous contact with strong acids, strong bases, or steam above 121 °C can overwhelm even a hydrolysis-resistant PBT grade. In underhood connectors, peak air temperatures beyond the heat deflection temperature under load can promote creep and contact relaxation. For parts with inserted metal terminals, the mismatch in linear thermal expansion between unfilled PBT and copper-alloy conductors should be reviewed; the coefficient of linear thermal expansion for unfilled PBT is commonly cited in the range of 10 × 10⁻⁵ K⁻¹ to 12 × 10⁻⁵ K⁻¹ between 23 °C and 55 °C. If the component is exposed to brake fluid, transmission fluid, or alkaline cleaning solutions, chemical compatibility should be validated through immersion testing according to ISO 22088 or an equivalent OEM procedure. Published data for 201HR-specific retention after exposure to aggressive automotive fluids is limited, so component validation should include aged terminal-insertion retention and housing latch force measurements.
In production-scale injection moulding of thin-wall connector housings, the material’s fast crystallisation can create a narrow holding-pressure window. Premature gate freeze is a known failure mode on multi-cavity tools with long cold-runner drops. Process engineers typically compensate with higher holding pressure and short hold-time transitions, but excessive packing can generate residual stress at the gate and reduce hydrolytic performance after ageing. Hot-runner systems with individually controlled nozzles are used when cavity-to-cavity fill variation exceeds dimensional capability limits. Melt residence time should be minimised because prolonged hold at melt temperature can deplete the stabiliser package and shift the material toward ordinary PBT-like behaviour. Scrap from hydrolytically stabilised PBT should not be blended into general-purpose PBT streams unless the receiving application tolerates altered melt-flow stability.