| HS Code | 367272 |
| Product Name | Trilene® TS 8058 |
| Manufacturer | Petroquímica Triunfo |
| Polymer Type | LLDPE-C6 and LDPE Blend |
| Comonomer | 1-Hexene |
| Density | 0.923 g/cm³ |
| Melt Index 190 C 2 16 Kg | 0.80 g/10 min |
| Melting Point | 124 °C |
| Vicat Softening Point | 100 °C |
| Tensile Strength At Yield | 11 MPa |
| Tensile Strength At Break | 30 MPa |
| Elongation At Break | 800 % |
| Flexural Modulus | 260 MPa |
| Shore D Hardness | 50 |
| Dart Drop Impact | 150 g |
| Elmendorf Tear Strength Md | 250 g |
| Elmendorf Tear Strength Td | 350 g |
| Haze | 12 % |
| Gloss 45 | 60 |
| Coefficient Of Friction | 0.15 |
As an accredited Petroquimica Triunfo Trilene® TS 8058 LLDPE-C6 and LDPE Blend factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Petroquimica Triunfo Trilene® TS 8058 comes in 25 kg polyethylene bags, palletized with 40 bags per pallet, totaling 1,000 kg. |
| Container Loading (20′ FCL) | Container Loading (20′ FCL): Petroquimica Triunfo Trilene® TS 8058 LLDPE-C6/LDPE blend, palletized, moisture-protected, weight-balanced, and securely stowed for ocean export. |
| Shipping | Petroquimica Triunfo Trilene® TS 8058 LLDPE-C6/LDPE Blend is shipped as a non-hazardous thermoplastic resin in 25 kg polyethylene bags, octabins, or bulk containers. Keep dry, away from heat, sunlight, and contamination. No UN/DOT hazard class required. Follow local transport regulations and safe handling practices. Store in cool, ventilated areas. |
| Storage | Store in a cool, dry, well-ventilated warehouse in original, sealed packaging. Keep away from direct sunlight, moisture, heat, flames, and strong oxidizers. Protect from UV light and ignition sources. Maintain ambient temperature; avoid prolonged exposure above 50 °C. Prevent dust accumulation and stacking damage. Use first-in, first-out inventory. Keep containers closed, clearly labelled, and follow the safety data sheet. |
| Shelf Life | Shelf life: typically 12 months when stored unopened in a cool, dry, ventilated place away from direct sunlight and moisture. |
Trilene® TS 8058, a C6 linear-low-density polyethylene and low-density polyethylene blend, is fed to the core and outer layers of a three-layer cast stretch film line. In the core layer, the blend is incorporated at 82–90 wt% with 10–18 wt% EVA-based cling masterbatch; in the two outer layers, the blend is dosed at 68–75 wt% with 25–32 wt% cling masterbatch containing 8–12 wt% polyisobutylene tackifier. On a production line with 75 mm and 120 mm extruders at 30:1 L/D, melt temperature is held at 240–260 °C, die temperature 245–255 °C, and chill-roll temperature 18–22 °C. Line speeds of 300–450 m/min produce films between 8 µm and 23 µm. Neck-in at the die exit is controlled to 15–25 mm, and edge trim is reintroduced into the core layer at up to 10 wt% without measurable gel formation. Puncture resistance is evaluated under ASTM D5748-19, cling under ASTM D5458-95(2020), and tensile properties under ISO 527-3:2018. Regulatory status is assessed against REACH 1907/2006; the grade is intended for non-food logistics wrap, and direct food contact would require end-use migration testing under EU Regulation 10/2011 and FDA 21 CFR 177.1520. Terminal products include machine-grade pallet wrap, pre-stretched hand wrap for beverage multipack unitization, printed bundling film, and non-cling interleaving film used in appliance logistics.
In heavy-duty sack converting, the film is extruded from a three-layer blown line with die diameter 160–250 mm, die gap 1.0–1.4 mm, and blow-up ratio 2.0–3.5. The melt profile is held between 170 °C and 210 °C, with internal bubble cooling maintaining frost line height 450–600 mm. The formulation contains 80–90 wt% Trilene® TS 8058, 10–20 wt% additional LDPE for bubble stability and heat-seal latitude, and 2–4 wt% carbon black/UV masterbatch for outdoor stockpile resistance in 25–50 kg export sacks. Film thickness ranges from 100 µm to 175 µm. Converted sacks are filled on form-fill-seal lines at 160–190 °C jaw temperature and 6–12 s cycle time; hot-tack performance and seal cleanliness are assessed by ASTM F88/F88M-15 at 200 mm/min jaw separation. Drop impact qualification follows ISO 7965-2:1993; Elmendorf tear resistance uses ISO 6383-2:1983; dart impact uses ASTM D1709-16a; accelerated weathering is referenced to ISO 4892-2:2013 for UV-exposed export handling. Terminal products include valve sacks for resin pellet export, open-mouth sacks for fertilizers, form-fill-seal sacks for granulated petrochemical additives, and gusseted block-bottom sacks with sift-proof closures.
| Standard designation | Measurement or compliance boundary | Application context |
|---|---|---|
| ASTM D5748-19 | Protrusion puncture resistance of stretch wrap film | Cast stretch film |
| ASTM D5458-95(2020) | Peel cling of stretch wrap film | Cast stretch film |
| ISO 527-3:2018 | Tensile properties of film and sheeting | Cast stretch film, heavy-duty sacks, agricultural film |
| ASTM D1709-16a | Free-falling dart impact resistance | Heavy-duty sacks, agricultural film |
| ISO 7965-2:1993 | Drop testing of thermoplastic flexible sacks | Heavy-duty sacks |
| ASTM F88/F88M-15 | Seal strength of flexible barrier materials | Heavy-duty sacks, extrusion lamination |
| EN 13206:2017 | Thermoplastic films for agricultural and horticultural use | Agricultural silage and greenhouse film |
| ISO 21898:2004 | Flexible intermediate bulk container safety requirements | Woven polypropylene lamination |
| EU Regulation 10/2011 | Food-contact migration limits | Frozen-food packaging |
At coating thicknesses between 15 µm and 25 µm, the blend is applied onto 10–14 tapes per inch woven polypropylene fabric through a 105 mm 30D extruder at melt temperature 280–320 °C and die gap 0.6–0.8 mm. The laminator runs at 80–150 m/min with nip pressure 25–35 N/mm². Formulation is 85–95 wt% TS 8058 with 5–15 wt% LDPE to control draw resonance at reduced coating weights. Adhesion to the corona-treated woven substrate is monitored at 38–42 mN/m surface energy; peel adhesion is qualified under ASTM F88/F88M-15. Coating weight variation on production samples remains within ±1.5 g/m² at 120 m/min, while edge neck-in at the die is 20–30 mm. Compliance for flexible intermediate bulk container outer shells references ISO 21898:2004; mechanical strength after lamination is verified under ISO 527-3:2018 and ASTM D1709-16a. Terminal products include FIBC outer shells, roll goods for building wrap, industrial tarpaulin lamination, and taping film for PP woven sacks.
On agricultural silage film lines processing Trilene® TS 8058, die diameters of 160–250 mm, blow-up ratios of 2.2–3.2, and frost line heights of 450–600 mm are maintained with internal bubble cooling. The blend is fed at 70–85 wt% with 15–30 wt% additional LDPE to increase bubble stability at low gauge; UV stabilization is provided by 4–8 wt% HALS/benzophenone masterbatch, and 2–5 wt% EVA is incorporated for silage-wrap puncture tolerance. Melt temperature is held at 190–220 °C, die gap 1.0–1.6 mm, and film thicknesses range from 25 µm to 200 µm. The resulting film must conform to EN 13206:2017 for agricultural thermoplastic covers, with tear resistance measured by ISO 6383-2:1983, dart impact by ASTM D1709-16a, and tensile by ISO 527-3:2018. In field-scale operation, frost line variation greater than ±50 mm produces local gauge bands that reduce silage bag tear resistance; die lip cleaning is required at 8–12 h intervals when UV masterbatch residues create oxidized edge particles. Terminal products include silage storage bags, stretch silage covers, greenhouse covering film, low-tunnel film, and fumigation barrier covers.
When frozen-food vertical form-fill-seal lines downgauge below 40 µm, a reduction in LDPE fraction to 12 wt% in the cold-temperature layer changes the film's low-temperature stress-response line, with failure mode distribution evaluated by ASTM D3420-14 at −20 °C. The balanced formulation uses 88 wt% Trilene® TS 8058 and 12 wt% LDPE, processed through a 0.8–1.2 mm die gap at melt temperatures 180–210 °C and BUR 2.2–2.8 to maintain MD/TD impact balance. Film thickness is 30–70 µm; sealing occurs at 120–150 °C with 0.5–1.0 N/mm² jaw pressure and 150–200 ms dwell. Direct food-contact eligibility requires end-use migration testing under EU Regulation 10/2011, with an overall migration limit of 10 mg/dm² under Article 12, and FDA 21 CFR 177.1520 olefin polymer clearance. Tensile and elongation before seal exposure are determined by ISO 527-3:2018. Published data for this specific blend in five-layer frozen-food structures is limited, but three-layer line production records show stable seal transfer at these parameters. Terminal products include frozen vegetable bags, French fry carton liners, ice packaging film, and fresh-produce overwrap with cold-chain distribution.
Collation shrink lines employ a blown film structure with the blend at 65–80 wt% and the balance LDPE at 20–35 wt% to achieve 70–80% transverse-direction shrink at 140–180 °C shrink-tunnel temperatures. Extrusion uses die diameter 150–250 mm, die gap 0.8–1.2 mm, blow-up ratio 3.0–4.5, and melt temperature 190–230 °C; high freeze-line extension at 600–800 mm sets TD orientation. Film thickness ranges from 30 µm to 80 µm, with MD shrink controlled to 15–25% to prevent bottle multipack distortion. Shrink tension and unrestrained linear shrinkage are evaluated under ISO 14616:1997 and ASTM D2732-14; tensile property after orientation is determined by ISO 527-3:2018. At production speeds above 60 packs/min, seal initiation must remain below 120 °C and hot-tack peel force above 2.0 N/25 mm at 110 °C to avoid end-seal pop-open; these thresholds are monitored on-line with package burst testers referenced to ASTM F1140/F1140M-13. Terminal products include collation wraps for bottled water, carbonated beverage can multipacks, sauce jar bundles, and shrink hood film used on palletized industrial goods.
Competitive Petroquimica Triunfo Trilene® TS 8058 LLDPE-C6 and LDPE Blend prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Petroquimica Triunfo Trilene® TS 8058 LLDPE-C6 and LDPE Blend is a formulated polyethylene system prepared from hex-1-ene linear low-density polyethylene and low-density polyethylene. The hexene comonomer introduces short-chain branches of six carbon atoms along the backbone, while the LDPE component contributes long-chain branching and a broad molecular weight distribution. The product is specified for blown-film extrusion and coextrusion applications in which bubble stability, dart impact resistance, and tear balance carry greater weight than maximum optical clarity. The model designation TS 8058 identifies a film-grade position within the Trilene portfolio; however, complete numerical release specifications for this specific blend are not publicly available, and converters must use the current Petroquimica Triunfo technical datasheet for exact density, melt mass-flow rate, and additive package. No independent verification of lot-specific values is supplied in this document.
Material classification follows polyolefin film-grade practice under ASTM D4976-12a and ISO 1872-1:2007. Incoming inspection typically includes density by ASTM D792-20, melt mass-flow rate by ISO 1133-1:2022 at 190 °C and 2.16 kg, and ash by ASTM D5630-13. The LDPE-rich phase lowers zero-shear viscosity and increases shear thinning, which reduces extruder backpressure and improves bubble stability on air-cooled blown-film lines. The C6-LLDPE phase increases tie-molecule formation relative to C4-LLDPE and contributes higher dart impact and improved Elmendorf tear propagation at equivalent film thickness. The blend ratio is the principal lever for adjusting shear viscosity; increasing LDPE content raises melt strength but also increases wide-angle haze and reduces transverse-direction tear.
At blown film start-up, the die gap is typically set between 1.5 mm and 2.5 mm for conventional LLDPE/LDPE blends, with a blow-up ratio of 2.0:1 to 3.0:1. Frost line height is adjusted between 0.4 m and 1.2 m according to film gauge and tower configuration. Exact values for TS 8058 should be derived from film thickness profiles and bubble temperature measurements on the target line. Melt pressure at the die entrance is monitored with a pressure transducer; an upward drift of more than 5% at constant screw speed suggests gel accumulation or feed-throat blockage. No processing-aid recommendation is made here because the formulation may already contain a slip and processing package.
Thermal stability boundaries follow conventional low-density polyethylene limitations. Barrel zones are typically set from 145 °C at the feed throat to 220 °C at the die adapter, with the die temperature held at 200–220 °C. Prolonged residence time above 240 °C accelerates chain scission and oxidation, leading to gel particles, oxidized specks, and reduced dart impact. The melt temperature measured at the die exit should remain below 220 °C unless the extruder and die are specifically designed for higher-temperature LLDPE processing. If the resin has been stored at relative humidity above 60% or in a condensing environment, pre-drying at 60 °C for 4 h may be applied to remove surface moisture, although polyethylene is not hygroscopic and internal moisture absorption is negligible.
Addition of an LDPE-rich phase shifts the shear-thinning onset to lower shear rates than that of neat C6-LLDPE. On a conventional monolayer blown-film line using a 50 mm grooved-feed extruder with a 24:1 L/D screw and a 200 mm spiral mandrel die, the pressure drop across the die is usually reduced by 5–15% relative to a similar melt-index C6-LLDPE control when the LDPE fraction is in a typical film-blend window. The long-chain branching relaxes more slowly in elongational flow; this property raises bubble stability but also narrows the shear-rate window before sharkskin melt fracture appears on the outer bubble surface. Die land length, die surface roughness, and output rate become first-order variables when the blend is operated below 190 °C or above a critical shear stress around 0.1–0.2 MPa for general-purpose LDPE-based blown-film systems. Product-specific critical shear stress for TS 8058 under industrial spiral-die conditions has not been published in accessible public sources; it should be determined on the target die profile using film inspection and surface profilometry.
Processors can delay melt fracture by increasing die temperature to 210–220 °C, reducing output, or widening the die gap. However, reducing the blow-up ratio or increasing the frost line height can destabilize the bubble if the LDPE fraction is low. Bubble stability is influenced by the strain-hardening behavior of the LDPE long-chain branches. The grade should therefore be evaluated with a time-lapse bubble position recorder or an ultrasonic layflat width sensor.
Stable operation is indicated by frost line height variation below ±5 mm and layflat width variation below ±2% over 30 min of continuous line output. These tolerances derive from blown-film practice for LDPE-rich blends; they must be revalidated on the specific air-ring, die-diameter, and internal-bubble-cooling configuration. The melt pressure profile should remain stable within ±1.0 MPa at constant die temperature. A rising pressure with constant throughput typically indicates gel accumulation on the screen pack or die surface. A falling pressure at constant screw speed may indicate feed disruption or melt channeling.
Because the blend contains both linear and long-chain branched polyethylene, gel formation can arise from either oxidative degradation or contamination with incompatible polymers such as polyamide, PET, or heavily filled masterbatch residues. The resin should not be combined with recycled material unless the recyclate has been screened for contamination levels below 500 ppm for non-polyethylene polymers and below 100 ppm for metal particles, depending on downstream film gauge and quality requirements. These limits are process-control guidelines from industrial film production and are not supplier-specific data.
The steady-state migration of slip and antiblock additives in this polyolefin matrix follows Fickian diffusion within the amorphous fraction. Because the LDPE-rich phase has lower crystallinity than the LLDPE-C6 phase and a higher free-volume fraction, additive migration to the film surface can be faster than in a neat C6-LLDPE film. This affects the coefficient of friction, measured by ASTM D1894-14, and blocking force, measured by ASTM D3354-15. A coefficient of friction below 0.3 after 24 h aging at 23 °C and 50% RH is commonly targeted for horizontal form-fill-seal lines. The target must be set by the converter because the additive package in TS 8058 is supplier-controlled.
Compliance assessment for food-contact or restricted-substance applications should use the following matrix.
| Parameter | Standard or regulation | Evaluation point |
|---|---|---|
| Density | ASTM D792-20 | Material classification and blend ratio |
| Melt mass-flow rate | ISO 1133-1:2022 at 190 °C/2.16 kg | Extruder throughput and viscosity screening |
| Film dart impact | ASTM D1709-22 | Gauge-normalized impact toughness |
| Elmendorf tear resistance | ASTM D1922-15 | Machine-direction and transverse-direction tear balance |
| Film haze | ASTM D1003-13 | Optical clarity of finished film |
| Vicat softening temperature | ASTM D1525-17e1 | Thermal resistance screening |
| Food-contact suitability | FDA 21 CFR 177.1520 and EU Regulation No 10/2011 | Migration testing and food-contact declaration |
| REACH | Regulation (EC) No 1907/2006 | SVHC candidate list declaration |
| RoHS | Directive 2011/65/EU Annex II and Commission Delegated Directive (EU) 2015/863 | Restricted substance compliance for non-food industrial use |
Because public documentation for the specific TS 8058 formulation is limited, using literature values for C6-LLDPE/LDPE blends should not be converted into acceptance criteria without supplier approval. The blend is not suitable for sustained service above 60 °C where creep and load-bearing stability are required, because low-density polyethylene loses modulus at elevated temperature. Applications requiring hot-fill above 80 °C should use a different polyolefin or confirm suitability through dynamic mechanical analysis and creep testing under ASTM D2990-17.
On production-scale lines, batch-to-batch variance in LDPE content can appear as changes in melt pressure, bubble stability, and film haze. A converter-side indirect control is to monitor melt flow ratio or shear viscosity ratio. For polyolefin film grades, an increasing melt flow ratio often corresponds to broader molecular weight distribution and higher long-chain branching. In-line rheometers or offline dynamic shear measurements under ISO 6721-10:2020 can quantify elastic modulus and phase angle; these are more sensitive to long-chain branching than melt mass-flow rate alone.
Dynamic oscillatory rheology of comparable C6-LLDPE/LDPE blends at 190 °C shows enhanced shear thinning with increasing LDPE content. The power-law index can decrease from approximately 0.6 for neat C6-LLDPE to below 0.4 at 20 wt% LDPE. Elongational viscosity rises more than shear viscosity, which is the key indicator of bubble stability. A Gottfert Rheotens or capillary breakup extensional rheometer is used to quantify melt failure and drawability. These data are class-level observations from polyolefin rheology and are not release specifications for TS 8058.
When hex-1-ene comonomer replaces but-1-ene in low-density blends, the optical and mechanical balance shifts. The C6 branch length allows more effective tie-molecule formation than C4 at equivalent density, improving dart impact and slow puncture resistance. The penalty is a slightly lower crystalline melting point and broader seal initiation range. In contrast, C8-LLDPE-based blends can show higher dart impact and better low-temperature seal initiation than C6 systems, but they may require higher melt temperatures or specialized screw designs and are generally more expensive. The LDPE fraction in TS 8058 differentiates it from neat metallocene C6-LLDPE because the long-chain branching improves melt strength and bubble stability but reduces transparency.
Compared with a conventional butene-based LLDPE/LDPE blend, a C6-based product such as TS 8058 is typically positioned for improved dart impact retention during downgauging. Compared with C6-LLDPE-only extrusion, the LDPE component lowers die pressure and increases bubble stability but reduces ultimate tensile strength and optical clarity. Compared with LDPE-only extrusion, this blend raises tensile strength and dart impact but reduces drawdown at high line speeds. Converter trials should quantify these differences on the target line with film gauge and output held constant.
Specific energy consumption in film extrusion of such blends typically ranges from 0.18 kWh/kg to 0.25 kWh/kg on air-cooled lines; sustained operation above 0.28 kWh/kg may indicate excessive shear heating, undersized dies, or high melt viscosity.
In heavy-duty shipping sacks, seal strength is tested by ASTM F88/F88M-15. Stable seal initiation at 115–130 °C is typical for C6-LLDPE-rich films, but actual values depend on density, LDPE content, and sealant-layer thickness. The sealant layer must be held below 130 °C to avoid film distortion if the outer layer is higher-temperature HDPE.
Coextrusion trials place TS 8058 as a core or skin component in multilayer structures. If the grade is used as a core layer, the outer skins may provide high gloss, low seal initiation temperature, or barrier properties. If used as a skin layer, the surface coefficient of friction and blocking behavior become critical. Film should be conditioned for 48 h at 23 °C before surface testing because additive migration is time-dependent. A change in film gauge from 50 µm to 25 µm should not be made solely by increasing blow-up ratio or frost line height; the resulting orientation and thickness-profile changes require re-qualification of tear and dart impact.
The product is not recommended for prolonged contact with strong oxidizing acids, chlorinated hydrocarbons, or halogenated solvents. Chemical resistance for specific packaging contents should be confirmed by ASTM D543-21. For outdoor storage, UV stabilization is not implied unless specifically stated by the supplier. Weathering performance should be verified by ASTM D4329-21 or ISO 4892-2:2020 if the film is exposed to direct sunlight beyond incidental exposure.