| HS Code | 433547 |
| Productname | NOVA Chemicals Sclair® 2318 LLDPE Injection Molding Resin |
| Manufacturer | NOVA Chemicals |
| Tradename | Sclair® |
| Productcode | 2318 |
| Polymertype | Linear Low Density Polyethylene (LLDPE) |
| Grade | Injection Molding Resin |
| Density | 0.924 g/cm³ |
| Meltindex | 50 g/10 min (190°C/2.16 kg) |
| Tensilestrengthatyield | 9.0 MPa |
| Tensilestrengthatbreak | 10.0 MPa |
| Elongationatbreak | 600% |
| Flexuralmodulus | 240 MPa |
| Vicatsofteningpoint | 88°C |
| Brittlenesstemperature | < -70°C |
| Hardnessshored | 50 |
| Typicalmelttemperature | 190-230°C |
| Typicalmoldtemperature | 20-50°C |
As an accredited NOVA Chemicals Sclair® 2318 LLDPE Injection Molding Resin factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | NOVA Chemicals Sclair® 2318 LLDPE Injection Molding Resin is supplied in 25 kg polyethylene bags, 40 bags per pallet (1,000 kg net). |
| Container Loading (20′ FCL) | Container loading (20′ FCL): NOVA Chemicals Sclair® 2318 LLDPE injection molding resin, 25 kg bags, palletized, shrink-wrapped, secured. |
| Shipping | NOVA Chemicals Sclair® 2318 LLDPE Injection Molding Resin pellets are supplied in 25 kg bags, octabins, or bulk hopper trucks/railcars. Store dry, clean, closed, away from heat, sunlight, moisture, and contaminants. Non-hazardous; use standard handling. Protect from punctures and temperature extremes. Transport in compliant, labeled containers; avoid contamination. |
| Storage | Store NOVA Chemicals Sclair® 2318 LLDPE resin in a cool, dry, well-ventilated warehouse. Keep containers sealed and off the floor, away from direct sunlight, heat, ignition sources, and oxidizing agents. Protect from moisture, dust, and contamination. Avoid excessive stacking or bag damage. Maintain moderate temperatures and follow the supplier SDS and local regulations. Use FIFO stock rotation. |
| Shelf Life | Shelf life is typically 24 months from manufacture when stored unopened in a cool, dry, ventilated area, away from sunlight and contaminants. |
Processing NOVA Chemicals Sclair® 2318 LLDPE injection molding resin in thin-walled food packaging begins from a nominal melt index of 18 g/10 min (ASTM D1238, 190 °C, 2.16 kg) and a nominal density of 0.930 g/cm³ (ASTM D792). In multi-cavity molds with sidewall stock between 0.45 mm and 1.20 mm, this viscosity window permits fill speeds of 150–300 mm/s without exceeding a melt temperature of 250 °C at the nozzle. Barrel set points on toggle-clamp machines in the 120–180 t range are staged at 180 °C in the feed zone, 210 °C in the compression zone, and 235 °C at the nozzle. The mold is controlled at 15–30 °C using turbulent-flow water lines, and the hold-pressure stage is set at 50–70 MPa for 0.5–1.2 s to compensate densification before gate freeze. The resin is not normally pre-dried when silo moisture is below 0.05 wt%, but surface condensation from cold pellets transferred in relative humidity above 80% can generate splay; in that condition a hopper dryer at 60 °C for 1 h is applied before processing. Terminal articles in this segment include 0.50–0.80 mm wall dairy tubs, dry-food snap lids, portion-cup overcaps, and rectangular meal-prep containers. The base resin is blended with food-contact-approved slip/antiblock masterbatch at 1–3 wt%, and when frozen-food impact resistance is required, a nucleating additive at 0.05–0.15 wt% is introduced to raise crystallization onset temperature and reduce post-crystallization shrinkage. Color concentrate is restricted to a PE carrier at addition levels below 4 wt%; higher loadings can reduce low-temperature dart impact under ASTM D3763 and may shift the failure mode from ductile tearing to brittle shatter at −20 °C. For food-contact articles, compliance is governed principally by FDA 21 CFR 177.1520 and EU Regulation No 10/2011. The overall migration limit under EU 10/2011 is 10 mg/dm² of food-contact surface, and extractive testing under FDA 21 CFR 177.1520 is conducted in n-hexane according to the food-type and temperature conditions specified by the regulation. Converters must verify that the selected masterbatch and colorant also meet the same migration criteria because additive migration is not governed solely by the base polyolefin.
| Regulatory framework | Provision | Test condition or simulant | Typical limit |
|---|---|---|---|
| FDA 21 CFR | 177.1520 | n-hexane extractables, food-type temperature table | Condition-dependent extractable ceiling |
| EU 10/2011 | Article 12 total migration | 10% ethanol, 3% acetic acid, 20% ethanol, 50% ethanol, vegetable oil | 10 mg/dm² food-contact surface |
| REACH | Annex XVII restricted substances | No migration of listed substances | Substance-specific |
| RoHS | Directive 2011/65/EU | Homogeneous material cadmium, lead, mercury, Cr(VI), PBB, PBDE | 0.01% or 0.1% by weight |
Overcap and closure molding with Sclair 2318 is not governed by injection speed alone; the dominant process defect is radial warpage caused by differential shrinkage between the hot gate region and the rapidly cooled rim. The nominal melt index of 18 g/10 min allows valve-gated hot-runner drops to fill 8–16 cavities at lower hydraulic pressure than a 10–15 g/10 min grade, but the same flowability reduces gate freeze time, requiring a hold-pressure profile that compensates for backflow while keeping core deflection below 0.05 mm across the sealing land. The barrel profile is staged at 190 °C feed, 215 °C compression, 230 °C metering, and 240 °C nozzle, with hot-runner manifold temperature held below 245 °C to avoid molecular weight reduction that changes cooling stress relaxation and increases installed camber of the overcap. Core and cavity surfaces are cooled at 10–25 °C, and conformal cooling around the gate insert is used to bring the gate region below crystallization onset temperature before ejection. The cooling time for an overcap sidewall of 1.0–1.5 mm is normally 5–9 s per cycle, after which clamp force is released and the part is ejected with air poppets to reduce push-pin distortion. Terminal products include dry-powder can overcaps, personal-care jar overcaps, and coffee-can snap-on closures, in which the retaining bead requires repeated removal and re-closure. The lower flexural modulus of this resin compared with HDPE is compensated by designing inward-facing retention tabs at 1.0–1.5 mm wall thickness. For non-food industrial overcaps, post-industrial regrind can be introduced up to 20% by weight only if the melt index shift is monitored by ASTM D1238 after every recycle pass; repeated heating at 230 °C can increase melt index by 1–3 g/10 min after three passes and narrow the processing window enough to affect gate seal. Food-grade versions of these closures are evaluated under FDA 21 CFR 177.1520 and EU Regulation No 10/2011, with special attention to the sealing land flatness because migration testing cannot correct a poor mechanical seal against the container rim.
Across housewares with wall stock above 2.0 mm, Sclair 2318 is processed under a different thermal condition than thin-wall packaging because cooling time becomes the dominant cycle element. Storage bin lids, drawer dividers, and under-bed storage shells are molded with tab or fan gates at lower injection velocities of 50–100 mm/s to avoid jetting, while the barrel is maintained at 180–220 °C to limit thermal degradation during longer residence times. The mold is split-level controlled: the cavity side is maintained at 20–30 °C for surface gloss, and the core side is held at 40–50 °C to reduce thermal gradient-induced bowing. Ejection is initiated only when the core-side surface temperature measured by infrared pyrometry falls below 75 °C, because hot-core ejection causes push-pin puncture and post-mold warpage that cannot be corrected downstream. Hold pressure is applied for 6–12 s to control sink depth below 0.03 mm on visible surfaces, and the clamp-force requirement is estimated at 0.4–0.6 t/cm² of projected shot area for conservative tool protection. For outdoor storage boxes, a UV masterbatch with hindered amine light stabilizer at 0.15–0.30 wt% active content is added; phenolic antioxidant loading is kept below 0.10 wt% to prevent gas-yellowing in enclosed storage environments. The base resin is frequently combined with regrind from cold-runner spruce and rejected parts at levels up to 15%, provided that the in-house melt index remains within 16–20 g/10 min under ASTM D1238. Terminal parts are tested for flexural modulus under ISO 178 and notched Izod impact under ASTM D256; the notched Izod value may demonstrate partial or no-break behavior at 23 °C, but the practical design limit is not strength-based because excessive creep of the storage shell under sustained load is the more common failure mode. The low-temperature performance of these housewares is evaluated by conditioning at −20 °C for 24 h and then subjecting the part to a 1.0 m drop impact; this procedure is more representative than coupon testing because cooling-rate-induced skin-core morphology controls impact energy absorption in thick sections.
Toy and juvenile product components impose a specification that is not limited to tensile or flexural strength; the resin must survive repeated exposure to surfactants, oils, and oral-contact simulants without developing stress cracks at molded-in snap features or metal inserts. Sclair 2318 exhibits the expected environmental stress-crack resistance advantage of a low-density PE backbone over HDPE, but the actual resistance is strongly dependent on molded-in stress and cooling rate. Parts are molded with slower fill speeds of 30–60 mm/s and generous radii of 1.5 mm at all reentrant corners to avoid stress concentrations that would shorten ESCR under service conditions. The mold is held at 25–35 °C, and packing pressure after gate freeze is limited to 40 MPa to reduce frozen-in stress while maintaining dimensional repeatability. ESCR testing is commonly specified under ASTM D1693 condition B in 100% Igepal CO-630 for >100 h without cracking, but published data for Sclair 2318 under specific toy production conditions is limited; each production lot must be qualified before release. Mechanical fasteners are assembled after a 48 h post-molding relaxation period to allow normal shrinkage compensation and to prevent stress cracking during screw insertion. Color concentrates for play products are formulated on EVA or PE carriers at addition rates below 4 wt% because excessive pigment loading can reduce instrumented impact energy under ASTM D3763 and produce visible stress whitening at gate vestiges. Juvenile products are assessed under the US CPSC and EN 71-3 for migration of certain elements, and the base resin must not contain intentionally added heavy metals; the final article must meet the soluble-element limits defined by EN 71-3 for the applicable toy category. Terminal products in this segment include doll furniture, play kitchen lids, toy storage figures, and building-block accessories in which the soft-touch ductility of the resin prevents sharp-edge fracture after repeated drops onto hard surfaces.
Where a flexible annular part must be forced over a metal spigot at sub-zero temperatures, the processing discipline for Sclair 2318 shifts from cycle-time reduction to molecular orientation control. Flexible industrial caps, hydraulic fitting protectors, and low-pressure nozzle adapters are injection molded with annular sections between 0.80 mm and 1.60 mm; these geometries require a single sub-gate on a non-functional surface and injection velocities of 120–180 mm/s to avoid gas-burn at the knit line. The barrel profile is capped at 235 °C to limit thermal degradation in the thin annulus, and the mold is cooled at 12–20 °C to produce a fine skin layer that improves hoop stiffness without sacrificing low-temperature ductility. Ejection is delayed until 8–12 s of cooling has elapsed, because earlier ejection can tear the thin annular wall or leave permanent ovality that interferes with sealing on the spigot. Silicone-based mold release is avoided because it can alter surface energy if the part is later pad-printed or bonded to a mating gasket. Weld-line integrity in annular parts is evaluated by a ring-split test after conditioning at −20 °C for 4 h; fracture initiation outside the weld line is the acceptance criterion because weld-line failure in service creates a leakage path across the retaining bead. For applications near electrical equipment, the finished part is often required to meet UL 94 HB at the molded thickness, but this resin does not carry a universal UL card in all colorants; the molder must validate flammability with the specific final formulation. Industrial parts that will contact hydrocarbons or lubricating oils are further tested after 7 days immersion at 23 °C in the target fluid, with dimensional change measured according to ISO 62 or an internal equivalent; the selection of Sclair 2318 is justified only when the part is expected to experience intermittent contact rather than continuous submersion, because long-term hydrocarbon absorption can plasticize the surface and reduce the retention force on the spigot.
For lids and access panels on insulated cold-chain containers, the product specification is driven by the need to survive repeated flexing at freezer temperatures without surface fracture or gross deformation. Sclair 2318 is processed in these applications with a melt temperature of 215–235 °C and a mold temperature of 20–30 °C, because higher mold temperatures increase gloss but also extend the cycle time without improving low-temperature ductility sufficiently to justify the added cost. The gate is positioned away from the hinge or flexing line, because freezine-in molecular orientation near the gate can generate a brittle plane that cracks when the panel is opened at −20 °C. The lid thickness is commonly designed at 1.2–2.0 mm at the flexing zone and 2.5–3.5 mm across the sealing periphery, with a tapered transition between the two sections to reduce stress concentration. The hold-pressure profile is reduced in two stages from 50 MPa to 20 MPa to avoid overpacking the flexing zone, and the screw cushion is maintained at 3–6 mm to ensure consistent pack without excessive shear work. Cold-chain lids are often colored in high-opacity whites or chilled blues; the color concentrate is selected from a PE-based system with a melt index within 10–20 g/10 min of the base resin to avoid localized flow front velocity changes in the transition section. The final parts are conditioned at −20 °C for 8 h and then subjected to a cyclic flex test at 0.5 Hz over a 30° angular displacement; cracking or visible craze formation before 1,000 cycles is normally cause for rejection. Seal retention is checked separately by fitting the lid onto its container and storing at 4 °C for 24 h, after which the closure force must remain within specification when measured with a constant-rate compression tester. These parts are not normally used in hot-fill or high-temperature food-contact applications, because the upper continuous use temperature of the resin is below that of many polypropylene grades, and creep under load above 60 °C may cause gasket channel distortion.
Competitive NOVA Chemicals Sclair® 2318 LLDPE Injection Molding Resin prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
SCLAIR® 2318 is a linear low-density polyethylene injection molding resin supplied by NOVA Chemicals. The product is identified as a butene-based LLDPE with a nominal melt index of 18 g/10 min measured under ISO 1133-1:2022 or ASTM D1238 at 190 °C with a 2.16 kg load, and a nominal density of 0.924 g/cm³ determined by ASTM D792 or ISO 1183-1. The combination of high melt flow and low density is intended for thin-wall injection molded packaging, closures, housewares, and similar parts. The values apply to the resin as supplied and do not include the effects of colorants, additives, or regrind.
At production scale, the melt index and density indicate a polyolefin that fills thin sections at lower injection pressure than general-purpose LLDPE film or blow molding grades. Differential scanning calorimetry under ASTM D3418 typically shows a peak melt temperature between 122 °C and 126 °C, consistent with a butene-copolymer LLDPE of this density. The lower crystallinity relative to high-density polyethylene affects both mechanical stiffness and post-mold shrinkage.
The principal distinction is flow. The 18 g/10 min melt index is between 3 and 6 times higher than the 0.5–4.0 g/10 min range common for LLDPE film or blow molding grades. In injection molding, that difference translates to shorter fill times and the ability to fill wall thicknesses below 1.0 mm without raising melt temperature above 230 °C. Compared with HDPE injection grades of density 0.948–0.965 g/cm³, the 0.924 g/cm³ density reduces flexural modulus and heat deflection temperature but improves environmental stress crack resistance when evaluated under ASTM D1693. Compared with LDPE injection grades of similar melt index, the linear butene-copolymer architecture produces stronger shear thinning and a different balance of tensile yield, flexural modulus, and elongation. Processors should not assume that an LDPE grade of the same melt index will show the same screw recovery rate, pressure drop, or part shrinkage.
| Property | Representative value | Test method |
|---|---|---|
| Melt index, 190 °C; 2.16 kg | 18 g/10 min | ASTM D1238; ISO 1133-1:2022 |
| Density | 0.924 g/cm³ | ASTM D792; ISO 1183-1 |
| Tensile yield stress | 10 MPa | ASTM D638-14; ISO 527-2 |
| Elongation at break | >600% | ASTM D638-14 |
| Flexural modulus, 1% secant | 220 MPa | ASTM D790-17; ISO 178 |
| Hardness, Shore D | 50 | ASTM D2240 |
| Vicat softening temperature | 88 °C | ASTM D1525 |
| Brittleness temperature | <-75 °C | ASTM D746 |
These values are representative, not bilateral specification limits. Lot-specific certificates of analysis remain the controlling reference for production release and process capability studies.
On horizontal injection molding machines with clamp force ratings from 800 kN to 3,500 kN, barrel temperatures are typically profiled from 180 °C in the rear zone to 220 °C at the nozzle, with maximum melt temperature not exceeding 240 °C. Feed throat temperature should remain below 60 °C to prevent pellet bridging and screw slippage. Mold temperature is maintained between 10 °C and 40 °C; lower settings reduce cycle time in thin-wall parts but increase injection pressure and frozen-layer orientation. No predrying is required for sealed original packaging at relative humidity below 60%. If surface moisture is introduced by open storage or regrind, predrying at 70–80 °C for 2 h in a desiccant-bed dryer with a dew point of -30 °C or lower is adequate. Back pressure of 0.5–1.5 MPa and screw decompression of 2–5 mm control shot-weight variation and nozzle drool. Excessive decompression entrains air and can produce splay. Screws with an L/D ratio of 20:1 to 24:1 and compression ratio of 2.5:1 to 3.0:1 are standard for polyolefins; general-purpose screws are acceptable.
Although 18 g/10 min signals high fill speed, the melt index is measured at low shear and cannot by itself predict injection pressure. Capillary rheometry under ASTM D3835 is required for mold-specific gate and runner sizing. Apparent viscosity at 190 °C and 1,000 s⁻¹ for this class of LLDPE typically falls between 25 Pa·s and 45 Pa·s; published data for this specific configuration is limited. In cavities thinner than 0.8 mm, injection pressure can exceed 80 MPa. Minimum clamp force is calculated as cavity pressure in MPa multiplied by projected area in cm² multiplied by 0.1. For a cavity pressure of 40 MPa and a projected area of 500 cm², the minimum clamp force is 2,000 kN. Flow length-to-thickness ratios of 150:1 are achievable with high-flow LLDPE but depend on gate geometry, mold temperature, and injection speed. The linear backbone produces stronger shear thinning than branched LDPE of similar melt index; therefore, higher injection speeds reduce filling pressure more for this polymer than for an equivalent-melt-index LDPE. The frozen layer is thinner at high shear, increasing flow area, but local melt temperature should not exceed 260 °C.
Injected parts require venting equivalent to at least 0.02–0.05 mm land depth on polyolefin molds to prevent diesel effect and burn marks; inadequate venting manifests as black deposits at the end of fill. Cavity pressure sensors placed near the gate and at end-of-fill allow transfer from velocity to pressure control before cavity pressure exceeds 60 MPa. These sensors also verify gate freeze time. In multi-cavity tools with hot-runner manifolds, the high flow index reduces pressure drop across the manifold, but small gate diameters may still require manifold temperatures near 220 °C to prevent premature gate freeze. Manifold temperatures above 230 °C increase the risk of resin degradation and black speck formation.
Tensile yield stress is approximately 10 MPa, with elongation at break typically above 600% when tested at 50 mm/min on Type IV specimens per ASTM D638-14. Flexural modulus, measured as the 1% secant value under ASTM D790-17, is typically 220 MPa. This low modulus permits easy demolding and flexibility in thin-wall containers but limits load-bearing stiffness relative to high-density polyethylene. Notched Izod impact specimens under ASTM D256 frequently show partial break rather than complete break, so the resulting values should not be treated as fracture mechanics parameters. Dart or instrumented puncture testing is preferred for drop-impact packaging. Low-temperature brittleness below -75 °C under ASTM D746 indicates ductile behavior in freezer environments, but sharp corners, weld lines, and orientation can reduce practical impact resistance. Weld lines formed by opposing flow fronts reduce elongation and impact strength; gate placement should locate weld lines away from sealing beads or load-bearing regions.
Linear mold shrinkage for SCLAIR® 2318 is typically 1.5% to 2.5% in the flow direction and may be 0.3% to 0.8% lower in the transverse direction because of anisotropic orientation. This differential is a primary cause of post-ejection warpage in flat lids and containers. Mold cooling circuits must maintain cavity surface temperature differentials of less than 5 °C; larger differences produce in-mold temperature gradients that persist as residual stress. Packing pressure should be held until gate freeze; premature gate freeze creates sink marks and variable shrinkage. Linear mold shrinkage values should be verified per ASTM D955. Gate location should generate a symmetric flow front because asymmetric filling creates orientation gradients that cannot be corrected by cooling alone. Gate land length and diameter should be sized to avoid early freeze in thin-wall tools. The molecular architecture of this high-flow LLDPE supports rapid solidification, but flatness should be verified on the actual tool because published data for this specific configuration is limited.
Compliance is use-specific and depends on additives, colorants, and regrind. Polyethylene copolymers of this density are referenced in FDA 21 CFR 177.1520; finished articles must meet extractive limitations in 21 CFR 176.170(c). In the European Union, plastic food-contact materials are regulated under Commission Regulation (EU) No 10/2011, with an overall migration limit of 10 mg/dm² and specific migration limits for monomers and additives. A NOVA Chemicals food-contact statement should be obtained for the specific grade and supply chain before commercial use. The resin is not intended for medical implant applications, and continuous use at sterilization temperatures above 121 °C is outside the normal design window.
| Framework | Scope | Relevant clause or limit |
|---|---|---|
| FDA 21 CFR 177.1520 | Olefin polymers for food contact | 21 CFR 176.170(c) extractive limits |
| EU Regulation 10/2011 | Plastic food-contact materials | Overall migration limit 10 mg/dm² |
| REACH | SVHC screening | EC 1907/2006 candidate list |
| RoHS | Hazardous substances in electrical and electronic equipment | Pb, Hg, Cr(VI), PBB, PBDE 0.1 wt%; Cd 0.01 wt% |
Thermal degradation during molding is governed by residence time and temperature. At melt temperatures above 240 °C, chain scission and oxidation increase; above 300 °C, degradation is rapid and produces carbonyl species, discoloration, and viscosity change. If a production interruption occurs, barrel temperatures should be reduced to 150 °C or the screw purged with a low-melt-index HDPE or acrylic purge compound. The melt should not be combined with strong oxidizing agents, chlorinated solvents, or unsaturated oils under heat or stress. Regrind from sprues and runners may be added up to 20 wt% when dry and free of contamination; higher levels require verification of viscosity and impact stability. These boundaries are standard for LLDPE injection molding grades and should be confirmed against lot-specific certificates of analysis.