| HS Code | 547803 |
| Polymer Type | Butene Linear Low Density Polyethylene (LLDPE) |
| Comonomer | Butene |
| Density | 0.920 g/cm³ |
| Melt Index | 0.75 g/10 min |
| Melting Point | 122 °C |
| Vicat Softening Point | 102 °C |
| Tensile Strength At Yield | 10.3 MPa |
| Tensile Strength At Break | 24.1 MPa |
| Elongation At Break | 800% |
| Tensile Modulus 1 Secant | 241 MPa |
| Dart Drop Impact | 120 g |
| Elmendorf Tear Strength Md | 360 g |
| Elmendorf Tear Strength Td | 480 g |
| Haze | 12% |
| Gloss | 60% |
As an accredited NOVA Chemicals Sclair® 11U4 Butene LLDPE Film Resin factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | NOVA Chemicals Sclair® 11U4 is supplied in 25 kg bags, 55 bags per pallet (1,375 kg), with bulk options. |
| Container Loading (20′ FCL) | 20′ FCL container loaded with 25 kg bags of NOVA Chemicals Sclair® 11U4 Butene LLDPE Film Resin, palletized and stretch-wrapped. |
| Shipping | NOVA Chemicals Sclair® 11U4 Butene LLDPE Film Resin is a non-hazardous solid pellet. It is shipped in 25-kg polyethylene bags, octabins, or bulk trucks/railcars. Keep containers clean, dry, and closed at ambient temperatures. Protect from moisture, contamination, and excessive heat. No special transport placarding or ventilation is normally required. |
| Storage | Store Sclair® 11U4 Butene LLDPE Film Resin in a cool, dry, well-ventilated area away from direct sunlight, heat, sparks, and flames. Keep containers closed and sealed to prevent moisture, dust, and contamination. Avoid prolonged UV exposure and excessive stacking pressure. Maintain clean, dedicated storage; follow manufacturer’s SDS and local regulations. Keep away from strong oxidizers. Use first-in, first-out inventory. |
| Shelf Life | Typically 12 months from date of manufacture when stored unopened in a cool, dry, clean area away from direct sunlight. |
NOVA Chemicals Sclair® 11U4, a butene linear low-density polyethylene film resin with a nominal density of 0.918 g/cm³ (ASTM D1505) and a melt index of 4.0 g/10 min (ASTM D1238 at 190 °C/2.16 kg), is converted as a monolayer cast film for machine-grade pallet stretch wrap in the 12–30 µm gauge band. The 4.0 g/10 min melt index falls into the lower-viscosity end of the cast-film processing window, permitting drawdown on high-speed lines without the high melt pressure penalties observed with fractional-melt resins. The butene branch structure yields ethyl side branches that are shorter than the butyl or hexyl branches introduced by hexene and octene comonomers; this reduces melt elasticity and permits stable web formation at die lip gaps as narrow as 0.5 mm. In monolayer stretch packaging, the resin is specified for pallet loads where pre-stretch ratios remain below 250%; machine rolls produced from 11U4 are applied with automatic turntable wrappers and rotary arm wrappers. The surface coefficient of friction is governed by the slip and antiblock additive package. Published supplier data for this grade identify cast film as the intended conversion route.
Formulation for a 20 µm monolayer cast stretch film typically uses 100 parts of 11U4, 0.5–1.2 wt% of polyisobutylene cling additive when surface tack greater than 0.30 kinetic COF is required, and 0.2–0.8 wt% of a 10% erucamide slip masterbatch only when the machine film must display release at the outer wrap layer. The same film can be produced without additional cling agent when the converter adjusts die lip temperature and chill roll temperature to produce surface crystallinity that stabilizes unwind tension. For pre-stretched machine wrap, no high-pressure LDPE is added because dilution with long-chain branched polyethylene reduces the strain-hardening plateau and lowers the 50% elongation load by a measureable amount in ASTM D882 tensile testing. Where a soft cling layer is required, the film is coextruded as an A/B/A structure in which 11U4 occupies the core and release skin layers at 70–80% of total thickness, while the cling skin layer carries the polyisobutylene additive.
On production-scale cast film lines, 11U4 is processed with smooth-bore extruders using L/D ratios from 28:1 to 32:1 and barrier screws with Maddock mixing sections. Melt temperatures at the die lip are maintained in the 246–260 °C range to balance drawdown against oxidative degradation; residence time below 8 min at the maximum setpoint reduces gel formation. The die gap is set from 0.5–0.9 mm, and the web is fixed to a polished chill roll at 18–32 °C. Air knife pressure between 4 bar and 8 bar is used to eliminate boundary-layer turbulence and prevent edge curl. Below 15 °C chill roll temperature, field observations report higher film blocking on the roll and unstable unwind tension after 24 h of storage. Edge pinning by electrostatic pinning or vacuum box is required above 120 m/min line speed; without it, neck-in across the die width can exceed 15% and reduce usable web width. The table below lists the typical processing envelope for monolayer cast film equipment.
| Processing zone | Lower setpoint | Upper setpoint | Unit |
|---|---|---|---|
| Barrel zone 1 | 177 | 204 | °C |
| Barrel zone 2 | 204 | 232 | °C |
| Metering zone | 232 | 260 | °C |
| Adapter and die | 232 | 288 | °C |
| Chill roll | 15 | 40 | °C |
| Die gap | 0.5 | 0.9 | mm |
| Line speed | 150 | 400 | m/min |
Operational boundaries must be set for die-lip deposit control. When line speed exceeds 350 m/min without extraction, low-molecular-weight species accumulate at the die lip and cause melt fracture streaks. If the chill roll surface roughness exceeds Ra 0.25 µm, the outer-wrap coefficient of friction variation expands beyond ±0.05, which leads to pallet wrap failures on automatic wrappers. The butene LLDPE platform also exhibits lower puncture propagation resistance than octene LLDPE at equivalent gauge; converters that claim high puncture service for 20 µm cast film must test according to ASTM D5748 because published data for this specific configuration is limited.
In frozen food laminates, 11U4 is introduced as a sealant or bulk layer in a coextruded blown film web rather than as a stand-alone packaging film. A typical three-layer frozen vegetable pillow pack at 60 µm total thickness uses 11U4 in the sealant layer at 20–35% of total thickness, with a high-stiffness HDPE or PP core for puncture resistance and an outer skin layer for flexographic print receptivity. The sealant layer is dry-blended with 15–25 wt% high-pressure LDPE to reduce seal initiation temperature and broaden the hot-tack plateau on vertical form-fill-seal machines running at 80–120 cycles per minute. Without the LDPE addition, the hot-tack strength of a butene LLDPE sealant web can drop below 1.0 N/25 mm within 150 ms of seal jaw opening, causing headspace leakers in frozen vegetable packs stored at -25 °C. Heat seal strength is validated by ASTM F88, and hot-tack by ASTM F1921.
Direct food contact compliance is anchored to FDA 21 CFR 177.1520 for olefin polymers and to EU Regulation (EU) No 10/2011 as amended. The converter must validate overall migration under the intended frozen-food condition using food simulant D1 for aqueous foods or simulant A for fatty foods; the EU overall migration limit is 10 mg/dm². If a pigmented masterbatch is used in a printed or white sealant layer, the colorant carrier must conform to FDA 21 CFR 178.3290. The table below summarizes the regulatory matrix for this application.
| Standard or regulation | Scope | Relevant condition |
|---|---|---|
| FDA 21 CFR 177.1520 | Olefin polymers in food contact | Conforms as a copolymer of ethylene and butene |
| EU 10/2011 | Plastic food contact materials | Overall migration limit 10 mg/dm² |
| FDA 21 CFR 178.3290 | Colorants for polymers | Applies only if pigmented masterbatch is used |
| REACH | Chemical registration | SVHC certificate from masterbatch suppliers |
Blown film processing for 11U4 in this laminate uses a die gap of 1.2–1.8 mm, blow-up ratio 2.0–3.0, and melt temperature 190–220 °C. Corona treatment of the sealant surface is set to 38–40 mN/m (ASTM D2578) before lamination to solventless adhesive, but only after the film surface has cooled to below 35 °C to prevent migration of erucamide species into the adhesive interface. Frost line height is held in the upper third of the bubble to minimize quench-related haze in the deep-freeze package. The terminal converted product includes pillow packs for frozen mixed vegetables, frozen seafood, and portion-pack frozen dough.
For heavy-duty shipping sacks, 11U4 is processed as the outermost film ply on a woven polypropylene substrate or as a blown film liner for 25 kg polymer granule sacks and 40 kg chemical bags. The film layer is specified at 60–80 µm, and the converter blends 5–10 wt% high-pressure LDPE into the butene LLDPE to improve bubble stability on air-cooled blown film lines. Slip and antiblock masterbatch addition is held at 1.0–2.0 wt%; higher addition rates reduce bag-to-bag friction below 0.25 kinetic COF and cause pallet instability during truck shipment. The outer film must retain a minimum kinetic COF of 0.25–0.35 (ASTM D1894) to keep stacked sacks from shifting on polyethylene stretch-wrapped pallets. Terminal products include valve bags for pelletized resins, open-mouth sacks for agricultural chemicals, and liner films for FIBCs.
The blown film conversion route uses a die gap of 1.8–2.4 mm, blow-up ratio 2.0–2.8, and melt temperature 195–215 °C. The bubble is stabilized with a dual-lip air ring and internal bubble cooling where available. The critical service test is the ASTM D1709 dart impact drop at -20 °C. For a 60 µm film, converters must validate that the dart value exceeds the sack buyer's specified threshold, commonly 600 g for polymer granule sacks; published data for this specific configuration is limited because dart impact depends on frost line cooling rate and film orientation. If validation fails, the converter either increases gauge to 80 µm or replaces part of the butene LLDPE with octene LLDPE, which raises the puncture and impact plateau but reduces output due to higher melt viscosity. Compliance for industrial chemical sacks is limited to REACH SVHC certification and packaging waste directive 94/62/EC heavy metal limits; FDA food contact compliance is not automatically transferable.
Institutional can liners and refuse sacks represent a low-complexity conversion for 11U4 in which the resin is dry-blended with 10–20 wt% post-industrial recycled butene LLDPE and 1.0–2.0 wt% carbon black masterbatch on a grooved-feed blown film line. Film gauge ranges from 25–40 µm; die gap is set at 1.8 mm, blow-up ratio at 2.0–2.5, and melt temperature at 180–210 °C. A 2.0 wt% carbon black addition is sufficient for opacity and ultraviolet screening in short-term waste holding, but long-term outdoor storage of black refuse sacks is not recommended because the butene LLDPE backbone loses elongation under solar loading. Terminal products include 60 L to 120 L bin liners, janitorial sacks, and contractor debris bags. Compliance is confined to REACH, CONEG heavy metal restrictions, and national packaging waste regulations; direct food contact authorization is not claimed for this formulation.
Stretch hood film lines running 11U4 require a split coefficient of friction design because the outer surface of the hood must slide over palletized goods during application, while the inner surface must grip the pallet load after recovery. In a three-layer cast coextrusion, 11U4 occupies the core at 70–80% of total thickness; the outer release skin contains 2.0–3.5 wt% of a combined slip and antiblock masterbatch; the inner cling skin is dosed with 1.0–2.0 wt% polyisobutylene or an ultra-low density ethylene copolymer to raise kinetic COF into the 0.45–0.60 range (ASTM D1894). The outer surface kinetic COF is controlled to 0.25–0.35 to prevent drag marks on corrugated cartons. The film gauge for automatic stretch hood machines is 80–150 µm, and the layflat width is cut to 500–1500 mm according to hooder frame configuration.
Cast coextrusion processing requires a die gap of 0.6–1.0 mm and melt temperatures at the die lip of 240–270 °C. The chill roll temperature is maintained at 15–22 °C to quench the film without producing blocking in the cling layer. If the inner cling layer exceeds 0.60 kinetic COF, roll storage above 40 °C for more than 48 h can create blocking that tears the film at unwinding. The terminal product is used on automated pallet hooders in building materials, beverage, and chemical distribution. Compliance is industrial packaging only: REACH and 94/62/EC heavy metal limits apply; neither FDA nor EU food contact status is automatically transferred. The main operational boundary is that butene LLDPE stretch hood film does not develop the same elastic recovery as octene-based grades at high pre-stretch ratios; converters that advertise recovery above 80% after 200% elongation must validate with ISO 527-3 hysteresis testing.
When the destination packaging is a silage bale wrap, 11U4 is compounded at the converter level because the base resin does not contain sufficient ultraviolet stabilizers for multi-month outdoor exposure. A typical silage wrap formulation uses 100 parts 11U4, 2.0–3.0 wt% of a UV masterbatch based on hindered amine light stabilizers and a benzotriazole UV absorber, and 6–10 wt% of a 60% titanium dioxide white masterbatch to reduce solar heat absorption and stabilize the baled feed temperature under black or white film. The film is extruded at 25–35 µm gauge on a cast line with a die gap of 0.9–1.2 mm and melt temperature 240–260 °C. Pre-stretch on the bale wrapper is limited to 55–70%; higher pre-stretch ratios thin the film below 20 µm and increase oxygen permeability above the threshold needed for anaerobic fermentation. Terminal products include 750 mm × 1500 m rolls for round balers and wider 500 mm rolls for square balers.
The relevant product standard is EN 14932, which governs thermoplastic stretch films for wrapping silage bales. Converters must document dimensional stability, elongation retention after weathering, and solar transmittance when black or white masterbatch is used. The operational boundary is 24-month outdoor storage: even with UV stabilization, butene LLDPE loses measurable elongation after two agricultural seasons, and film that must remain intact beyond 24 months should be evaluated with ISO 527-3 after 2000 h accelerated weathering. This film is not intended for direct food contact; compliance follows general REACH registration and national agricultural film disposal schemes.
Competitive NOVA Chemicals Sclair® 11U4 Butene LLDPE Film Resin prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
SCLAIR 11U4 is a butene linear low-density polyethylene film resin supplied by NOVA Chemicals for monolayer and coextruded blown film structures. The grade is defined by a nominal melt index of 1.0 g/10 min when determined by ASTM D1238 at 190°C under a 2.16 kg load and a nominal solid-state density of 0.920 g/cm³ when determined by ASTM D792. The butene comonomer introduces short-chain branching that reduces crystalline lamellar thickness, lowers flexural modulus, and shifts the melting endotherm below that of ethylene homopolymers of comparable molecular weight. Because the resin is produced with a multi-site catalyst system, the molecular weight distribution is broader than that of most metallocene-catalyzed LLDPE grades; this feature tends to improve bubble stability but lowers ultimate dart impact. The pellets are stabilized with a phenolic/phosphite antioxidant system, but the base stabilization does not include ultraviolet absorbers or hindered amine light stabilizers. The resin is supplied in free-flowing pellet form and is intended for gravimetric or volumetric dosing into a hopper blender with additive or color masterbatch.
Thermal analysis by differential scanning calorimetry shows a broad melting endotherm with peak melting temperature near 122°C to 124°C; crystallization temperature upon cooling at 10°C/min is typically 104°C to 106°C. Vicat softening temperature by ASTM D1525 is approximately 100°C. The crystallization half-time at 110°C is longer than that of high-density polyethylene, which reduces cooling demand on the blown film line. Melt elasticity and bubble stability arise from a broad molecular weight distribution with a polydispersity index above 3.5, although the exact value is not published in the public datasheet. Melt strength at 190°C is sufficient for blow-up ratios up to 3.0:1; higher ratios can produce bubble sag and gauge variation. The resin is not formulated for high-melt-strength thermoforming or extrusion coating.
In blown film extrusion, the process window is bounded by melt temperature, die gap, and blow-up ratio. Melt temperatures between 190°C and 220°C are commonly maintained; the lower bound reduces thermal oxidation and gel formation, while the upper bound improves melt homogeneity in screw channels. Extruder configurations with 24:1 to 30:1 L/D and barrier screws with dispersive mixing elements are used to manage the shear sensitivity of butene LLDPE. Melt pressure at the die should remain within the manufacturer's rating; if wall shear stress exceeds approximately 0.14 MPa, sharkskin surface melt fracture becomes visible. For gauge below 25 µm, a fluoropolymer processing aid at 200 ppm to 800 ppm may be required to lower die stress and maintain bubble stability. Die gaps between 1.5 mm and 2.5 mm are standard; narrower gaps improve gauge uniformity but increase shear heating and can initiate degradation if melt temperature exceeds 220°C. Blow-up ratio is typically set from 2.0:1 to 3.0:1. Frost line height of 2 to 4 die diameters balances machine-direction and transverse-direction orientation. Output is limited by bubble instability below 25 µm, not by screw recovery in most 45 mm to 75 mm extruders; internal bubble cooling or a higher-melt-strength skin layer is required for thin-gauge production. Barrel temperature profiles commonly start with a feed zone at 140°C to 160°C, progress through compression at 180°C to 200°C, and hold metering at 190°C to 210°C; the die is maintained at 200°C to 210°C to minimize weld lines.
Film mechanical properties are thickness-dependent and strongly influenced by cooling rate. At 25 µm to 50 µm, machine-direction elongation at break typically exceeds 500% by ASTM D882; transverse-direction elongation is usually 100 to 200 percentage points higher because of transverse orientation. Elmendorf tear strength by ASTM D1922 is anisotropic: machine-direction values are 30% to 50% lower than transverse-direction values at 25 µm. Dart impact by ASTM D1709 method A for this butene resin class at 25 µm is commonly 80 g to 120 g. This places the grade below the typical threshold for aggressive frozen-food packaging, where a minimum dart impact of 150 g at 25 µm is often specified. Haze measured by ASTM D1003 is typically 12% to 15%, and 60° gloss by ASTM D2457 is typically 55 to 65. These optical values are within the general-purpose liner, produce bag, and garment overwrap range, but not in high-clarity or shrink-label applications. Puncture resistance should be verified by ASTM D5748 before use in heavy industrial sacks or construction film. Low-temperature brittleness by ASTM D746 is below -70°C, but low-temperature puncture should not be inferred from brittleness alone.
Hexene and octene LLDPE resins of equivalent melt index and density produce a higher tie-molecule fraction because the longer alpha-olefin branches are less efficiently incorporated into the crystalline lattice. The consequence is that Sclair® 11U4 usually requires 10% to 25% greater thickness to match the dart impact and puncture resistance of a hexene LLDPE film. Class-level blown film data show that hexene LLDPE at 0.920 g/cm³ and 1.0 g/10 min can exhibit 50% to 100% higher dart impact and 20% to 60% higher machine-direction Elmendorf tear than butene LLDPE. Octene LLDPE widens the difference further, particularly in low-temperature puncture. Conversely, butene LLDPE of equal melt index tends to have lower melt viscosity at the same temperature, which can reduce extruder torque and permit higher throughput on torque-limited lines. The lower comonomer cost of butene may reduce resin cost per kilogram, but the converter must evaluate total packaged cost after accounting for any required gauge up-weighting. Die gap, blow-up ratio, and frost line height interact with comonomer type; a substitution that retains the same processing conditions will usually shift the MD/TD property balance and may create film wrinkles or blocking. Metallocene butene grades may offer better clarity and dart impact at equivalent density, but they can require narrower melt temperature control and may be more sensitive to shear-induced melt fracture.
| Property at 25 µm | Butene LLDPE class | Hexene LLDPE class | Octene LLDPE class | Test Method |
|---|---|---|---|---|
| Dart impact | 80–120 g | 150–250 g | 200–300 g | ASTM D1709A |
| Machine-direction Elmendorf tear | 150–250 g | 300–450 g | 350–500 g | ASTM D1922 |
| Low-temperature puncture | lower | higher | highest | ASTM D5748 |
Published data for Sclair® 11U4-specific comparative film measurements are limited; the ranges in Table 1 are class-level values drawn from polyolefin film literature and should be confirmed on the target extrusion line before specification decisions are finalized.
Additive interactions and regrind behavior require line-specific validation. Slip agents such as erucamide migrate at a rate dependent on film crystallinity; at 0.920 g/cm³, migration is slower than in lower-density resins, so blocking can persist for several days after extrusion unless an antiblock masterbatch is used. Antiblock particle size should be between 2 µm and 6 µm to minimize haze while preventing blocking. Calcium stearate-based processing aids can interact with phenolic antioxidants and reduce color stability if dosed above 500 ppm. Clean regrind from Sclair® 11U4 film can be re-extruded at levels up to 20% without significant loss of mechanical properties; higher regrind fractions increase gel count and reduce dart impact. The exact regrind limit depends on screw design, melt filtration, and film thickness.
The resin may be evaluated for direct food contact under FDA 21 CFR 177.1520, which covers olefin polymers, provided that the final article meets end-use specifications and migration limits. In the European Union, compliance with Regulation (EU) No 10/2011 must be established through overall migration testing with a limit of 10 mg/dm² and specific migration limits for any monomers or additives present. The base polyolefin is not subject to authorization under REACH; registration status is confirmed in the safety data sheet issued by NOVA Chemicals. The resin contains a phenolic/phosphite stabilizer package; converters should avoid combining it with amine-based antistatic or slip concentrates that can deactivate the antioxidant system or produce yellowing. For fatty food contact, migration testing under OM2 or OM3 simulants is required. Ultraviolet resistance is not provided by the base stabilization; outdoor film requires a UV masterbatch at 2% to 5% by weight, but the exact dosage depends on the target exposure period and film thickness.
| Regulatory Document | Relevant Clause or Limit | Assessment Requirement |
|---|---|---|
| FDA 21 CFR 177.1520 | Olefin polymer specification | End-use testing and supply chain documentation |
| Regulation (EU) No 10/2011 | Overall migration 10 mg/dm² | Food simulant testing under OM2/OM3 |
| REACH | Registration dossier | Article/tonnage verification via safety data sheet |
On high-output cast film lines, melt temperature may reach 230°C, but residence time at temperature must be limited because butene LLDPE can generate gel particles from oxidative degradation above 240°C or during prolonged idle periods. Batch-to-batch melt index shifts greater than 0.1 g/10 min can alter bubble stability and gauge control; in-line rheometry or capillary rheometry at 190°C should be used to monitor incoming lots. Purging with a high-viscosity polyethylene after shutdown reduces carbon deposits at the die lip and prevents cross-contamination with higher-density resins. Film blocking can occur at gauge below 15 µm unless an antiblock masterbatch is added; silica or talc antiblock at 1000 ppm to 3000 ppm is typical, but the level must be balanced against haze increase. Low melt temperature operation below 180°C is not recommended because the high-molecular-weight fraction may not fully plasticate in shallow-groove feed sections, producing visible gels and poor web flatness.