| HS Code | 384864 |
| Polymer Type | Linear Low Density Polyethylene (LLDPE) |
| Comonomer | Octene |
| Density | 0.919 g/cm³ |
| Melt Index 190 C 2 16 Kg | 0.75 g/10 min |
| Melt Flow Ratio I21 I2 | 30 |
| Melting Point | 123 °C |
| Vicat Softening Point | 98 °C |
| Tensile Strength At Yield Md | 10.3 MPa |
| Tensile Strength At Break Md | 37.9 MPa |
| Tensile Strength At Yield Td | 10.3 MPa |
| Tensile Strength At Break Td | 30.3 MPa |
| Elongation At Break Md | 800% |
| Elongation At Break Td | 900% |
| 1 Secant Modulus Md | 220 MPa |
| 1 Secant Modulus Td | 260 MPa |
| Dart Drop Impact | 120 g |
| Elmendorf Tear Strength Md | 250 g |
| Elmendorf Tear Strength Td | 400 g |
| Haze | 10% |
| Gloss 45 | 65 |
As an accredited NOVA Chemicals Sclair® 11J4 Octene LLDPE Film Resin factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | NOVA Chemicals Sclair® 11J4 Octene LLDPE Film Resin is supplied in 25 kg polyethylene bags, typically palletized for shipment. |
| Container Loading (20′ FCL) | Sclair 11J4: 20′ FCL loads 20 pallets, 55 x 25 kg bags each, 27.5 MT net; shrink-wrapped and secured. |
| Shipping | NOVA Chemicals Sclair® 11J4 Octene LLDPE Film Resin ships as non-hazardous solid pellets in moisture-resistant 25 kg bags, palletized and stretch-wrapped, or in bulk containers/railcars. Transport in clean, dry trucks or railcars; protect from heat, moisture, and contamination. Not classified as dangerous goods. |
| Storage | Store Sclair® 11J4 LLDPE resin indoors in a cool, dry, well-ventilated area away from direct sunlight, heat, and ignition sources. Keep bags or containers closed, clean, and palletized off the floor. Protect from moisture, dust, and contamination. Avoid strong oxidizers. Maintain good housekeeping and first-in, first-out rotation. Do not store near odorous materials. Follow the manufacturer’s SDS and local regulations. |
| Shelf Life | Shelf life is 2 years from date of manufacture when stored in original packaging under cool, dry conditions away from direct sunlight. |
Cast stretch film lines producing machine pallet wrap at 500–900 m/min require an octene LLDPE with tension retention and puncture resistance sufficient for folded-pallet edge contacts. Sclair® 11J4, an octene LLDPE with a melt index of 1.0 g/10 min at 190°C/2.16 kg under ASTM D1238 and density of 0.918 g/cm³ under ASTM D792, is extruded in a three-layer A/B/C cast die with chill roll temperature 18–28°C, air gap 15–35 mm, and die lip gap 0.6–1.0 mm. The core layer receives 11J4 at 80–90 wt% blended with metallocene VLDPE at 10–20 wt%; the cling layer uses 11J4 at 15–30 wt% in a metallocene plastomer matrix, with polyisobutylene tackifier added at 0.5–2.0 wt%; the release layer blends 11J4 at 70–85 wt% with LDPE at 10–20 wt% and erucamide slip plus silica antiblock at combined 1,200–3,000 ppm. Extruders are single-screw machines with barrier screws and L/D 30:1, profiled from 170°C at the feed throat to 245–260°C at the die. Compliance for pallet wrap that may be placed adjacent to packaged food is governed by FDA 21 CFR 177.1520(c) for olefin polymers and EU Regulation 10/2011 for overall migration when indirect food contact is declared. Relevant film property tests include ASTM D5458 for cling, ASTM D5748 for puncture resistance, and ASTM D882 for tensile elongation at break. Terminal product types include 12–35 µm hand stretch, 17–35 µm machine stretch, and 40–60 µm heavy-gauge film for cornerboard and sharp-edged industrial loads. A production limitation observed on high-speed cast lines is unwind blocking when chill roll temperature exceeds 30°C and tackifier content is above 1.8 wt% without sufficient release-layer slip migration.
| Layer | Sclair® 11J4 (wt%) | Co-resins/additives | Test standard |
|---|---|---|---|
| Core | 80–90 | mLLDPE 10–20 wt% | ASTM D882 |
| Cling skin | 15–30 | mLLDPE plastomer 70–85 wt%, PIB 0.5–2.0 wt% | ASTM D5458 |
| Release skin | 70–85 | LDPE 10–20 wt%, slip/antiblock 0.12–0.30 wt% combined | ASTM D1894 |
On three-layer and seven-layer blown film lines running 11J4 in the two outer layers and a metallocene LLDPE in the core, the frost line height is typically set at 5–8 die diameters above the dual-lip air ring, with blow-up ratio held at 2.5:1–3.5:1 and die gap at 1.2–2.4 mm. In frozen-food packaging, the cooling rate difference between the outer and inner bubble surfaces creates crystallinity gradients that affect ASTM D1709 dart impact and ASTM D746 brittleness temperature. The formulation addition ratio for 11J4 in this segment is 65–85 wt% of the total polyethylene fraction, with LDPE or mLLDPE at 10–25 wt% and a fluoropolymer polymer processing aid at 0.02–0.06 wt% to suppress melt fracture during high-output runs. Silica antiblock and erucamide slip are added at combined 0.05–0.30 wt%, depending on gauge and film-to-film coefficient-of-friction targets measured under ASTM D1894. Extruder zones are profiled from 170°C at the feed throat to 210–230°C at the die, with melt temperature limited to 240°C to minimize degradation of the octene branches and gel formation. Terminal product types include 50–100 µm frozen vegetable pillow bags, 80–150 µm ice cream block pouches, and 100–180 µm seafood or bone-in meat shrink bags. Food-contact compliance is governed by FDA 21 CFR 177.1520 and EU Regulation 10/2011, with overall migration tested under conditions of use not exceeding 70°C for fatty simulants. Production bottlenecks observed on high-speed lines include dart impact losses above 25% when frost line height exceeds 10 die diameters, requiring air collar adjustment or blow-up ratio reduction.
In FIBC liner and industrial sack production on coextrusion blown film lines, Sclair® 11J4 is processed at 80–95 wt% blended with recycled LDPE at 5–15 wt% and carbon black UV masterbatch at 2–5 wt% for outdoor storage. The die gap is set between 1.8 mm and 2.8 mm for films as thick as 150–250 µm; melt pressure upstream of the screen changer is monitored at 250–350 bar, and screw speed is adjusted to maintain melt temperature below 245°C. The addition ratio of 11J4 at 75–90 wt% provides low-temperature flexibility and tear propagation resistance measured through ASTM D1922 Elmendorf tear and ASTM D1709 dart impact. In sack converting, the film is gusseted, surface treated to 38–42 dyn/cm via corona, printed flexographically, and welded with hot-bar or ultrasonic sealing at 40–70 m/min. Compliance standards for industrial sacks include ISO 21898 for flexible intermediate bulk containers where the liner acts as a dust barrier, and ASTM D882 for tensile yield stress. Terminal product types include 100–200 µm bulk container liners, 120–180 µm chemical shipping sacks, and 80–150 µm construction aggregate bags. Observed production failures include bubble instability at blow-up ratio above 3.0:1 when 11J4 content drops below 70 wt%, and low tear resistance when the recycled LDPE fraction exceeds 20 wt% due to broad molecular weight distribution.
Extrusion coating of paperboard for aseptic and gable-top liquid cartons uses Sclair® 11J4 as a heat-seal layer where octene LLDPE low seal initiation and puncture resistance extend shelf life under distribution compression. The resin is deposited through a slot die at 15–25 µm coating thickness onto paperboard at line speeds of 300–500 m/min, with melt temperature at 300–320°C, air gap 200–300 mm, chill roll temperature 15–25°C, and die deckle adjusted to control neck-in. Formulation addition ratio in the sealant layer is 11J4 at 80–100 wt%, with LDPE at 0–20 wt% to reduce neck-in and improve drawdown; adhesion to aluminum foil or paperboard is achieved through an ozone-treated LDPE tie layer applied at 20–40 g/m². For gable-top milk cartons, the sealant layer must meet FDA 21 CFR 177.1520(c) and EU Regulation 10/2011, with specific migration testing for octene oligomers conducted under EN 1186 and 10/2011. Terminal product types include 250 mL–1 L gable-top cartons for milk and juice, 500 mL–2 L aseptic brick packs, and liquid paperboard cups with lid-assist membranes. The processing window is constrained by seal initiation temperature: seal strength is tested at 140–160°C jaw temperature and 0.5 MPa pressure, with dwell time 0.5–1.0 s, and failure below 10 N/25 mm indicates insufficient sealing or contamination from paper dust. Published data for this specific grade in aseptic coating systems is limited, but sealant layer performance follows octene LLDPE extrusion coating practice.
Coextruded three-layer blown films for all-PE stand-up pouches place Sclair® 11J4 in the sealant layer and a higher-density PE in the stiff outer layer, with tie layers based on ethylene-vinyl acetate or maleic anhydride-grafted PE. The sealant layer thickness is typically 15–30 µm, at 11J4 addition ratio of 80–100 wt%, with anti-block silica at 0.1–0.4 wt% and slip at 0.05–0.2 wt% to prevent re-blocking after corona treatment. The blown film line uses a three-layer die with blow-up ratio 2.0:1–3.0:1, die gap 1.2–2.0 mm, and total film thickness 60–120 µm. The printed web is laminated to oriented HDPE or MDO-PE film via solventless adhesive at 1.8–2.5 g/m² coat weight, then converted into pouches at 40–80 cycles/min. Seal strength is measured according to ASTM F88/F88M-21, with target values above 12 N/25 mm at 140°C jaw temperature and 0.5 MPa pressure; below 15 µm sealant layer thickness, heat seal strength decreases due to partial mixing with the adjacent tie layer. Compliance is governed by FDA 21 CFR 177.1520 and EU Regulation 10/2011, with overall migration tested under EN 1186. Terminal product types include 500 mL–2 L laundry detergent refill pouches, 250 mL–1 L frozen beverage pouches, and 500 g–5 kg dry food stand-up pouches. Slip additive above 0.4 wt% should be avoided because seal strength falls below converting line peel thresholds.
Agricultural silage wrap and bale film use Sclair® 11J4 in cast film construction at 70–85 wt% with metallocene VLDPE at 10–20 wt% and a UV masterbatch at 5–10 wt% containing hindered amine light stabilizers at 0.3–0.8 wt% in final film. The film is produced on cast extrusion lines at 25–35 µm thickness, winder tension controlled to 15–25 N/m to maintain pre-stretch capability. Cling is generated by adding polyisobutylene at 0.5–2.0 wt% to one skin layer; high cling levels are necessary for 4–6 wrap layers around round bales at 50–70% pre-stretch. Compliance for agricultural films references EN 13206 for covering films and ISO 4892-2 for accelerated UV weathering. Oxygen transmission rate measured by ASTM D3985 is controlled by film thickness and orientation rather than resin alone. Terminal product types include 25 µm silage bale wrap, 35–50 µm silage bags, and 150–200 µm pond liners combining 11J4 with LDPE. Operational limits include UV masterbatch exceeding 12 wt% causing melt pressure fluctuations and die lines; storage above 35°C causes cling additive migration to the release surface.
Competitive NOVA Chemicals Sclair® 11J4 Octene LLDPE Film Resin prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
`NOVA Chemicals Sclair® 11J4` is a solution-polymerized linear low-density polyethylene film resin based on 1-octene comonomer. The grade is specified for cast and blown film structures in heavy-duty industrial liners, machine-grade stretch wrap, agricultural film, and regulated food-contact packaging. Two physical coordinates define the resin: a nominal density of 0.920 g/cm³ by ASTM D1505 and a nominal melt index of 1.0 g/10 min at 190 °C/2.16 kg by ASTM D1238. These values place the material in the intermediate-density LLDPE segment, where octene comonomer changes solid-state toughness and sealing behavior relative to butene LLDPE of similar melt index. The resin is supplied in pellet form for bulk railcar, octabin, or bag unloading and is not intended for injection molding, rotomolding, or pipe extrusion.
The comonomer effect arises from the length of the short-chain branch left after polymerization. Butene LLDPE carries ethyl branches, hexene LLDPE carries butyl branches, and octene LLDPE carries hexyl branches. At equal density and melt index, the longer branch in octene LLDPE increases the probability of tie-chain formation between adjacent crystallites, which raises energy dissipation under puncture and dart impact. Film processors evaluate this difference through ASTM D1709A dart drop on 25 µm blown film and ASTM D5748 puncture resistance on cast or blown film. Published data for `Sclair® 11J4` at all line configurations is limited, and comparative values must be confirmed on the target equipment because blow-up ratio, frost-line height, and die gap alter the balance of machine-direction and transverse-direction orientation. In production-scale evaluations, octene LLDPE of this density generally exhibits higher dart impact than butene LLDPE at the same gauge, but the magnitude of improvement is line-dependent and cannot be stated as a universal value.
On cast film lines, the grade is normally extruded at melt temperatures of 204–232 °C through a coat-hanger die with a die gap of 0.75–1.50 mm. Chill-roll temperatures in the range of 18–30 °C are used for thin gauges down to 12 µm. Melt curtain height and vacuum box settings require adjustment because the resin lacks the long-chain branching of high-pressure LDPE; neck-in is generally higher, and the melt curtain is more sensitive to air draft. Production-scale equipment with 24:1 to 30:1 L/D single-screw extruders and barrier screws having a compression ratio of 2.5:1 to 3.5:1 can provide adequate homogenization. Lines below 24:1 L/D may require elevated barrel temperatures or reduced screw speed to avoid unmelted regions, and melt filtration with screen packs of 80–120 mesh is typical for reducing gel-related film defects.
The base resin is supplied with a thermal stabilizer package intended for film extrusion. Most film grades in this class do not contain high levels of slip or antiblock as supplied; converters add a low-density polyethylene or LLDPE-based masterbatch at 2–4 wt% to target a coefficient of friction below 0.30 by ASTM D1894 after aging. Oleamide and erucamide slip additives migrate through the amorphous phase at rates dependent on film crystallinity, storage temperature, and film thickness. At 23 °C, a 25 µm cast film may require up to 48 h for stable coefficient-of-friction development; increasing storage temperature to 40 °C reduces this interval to approximately 24 h. Slip masterbatch additions above 5 wt% can produce chill-roll plate-out, die-lip buildup, and coefficient-of-friction inversion. Amine-based antifog concentrates should be evaluated for surface plate-out and for additive migration interactions because they can alter film friction after 48 h aging under ASTM D1894. Combinations with aggressive peroxide masterbatches should be limited to intentional reactive modification; residual free radicals can shift the melt index outside the 1.0 g/10 min specification and generate crosslinked gel particles.
The primary performance difference between `Sclair® 11J4` and a butene LLDPE of the same 0.920 g/cm³ density and 1.0 g/10 min melt index is not melt flow but impact-tensile balance. In laboratory comparisons using ASTM D882, octene grades generally show higher elongation at break and higher dart impact at 25 µm than butene grades, while butene grades may offer lower raw-material cost. Against high-pressure LDPE, `Sclair® 11J4` exhibits reduced melt tension, higher elongation at break, and a different heat-seal initiation plateau. Against metallocene LLDPE of comparable density, `Sclair® 11J4` may show lower optical clarity and lower dart impact but benefits from lower extrusion pressure and fewer melt fracture defects on narrow die gaps. These differences are structural and must be quantified on the specific film line because draw ratio, die gap, and chill-roll temperature alter the relative rankings.
Corona treatment is used to raise surface energy for printing and lamination. A 25 µm film treated at 0.5–1.0 kW·min/m² typically reaches 38–42 mN/m surface tension by ASTM D2578. Treatment intensity above 1.5 kW·min/m² may oxidize surface species and create low-molecular-weight oxygenated compounds that increase surface friction, reduce hot-tack force, and shift seal initiation temperature upward. Converters running high-speed vertical form-fill-seal lines should qualify heat-seal windows after corona aging because surface oxygen species can alter seal strength as measured by ASTM F88. On blown film lines, in-line corona treatment is often positioned after the collapsing frame; web tension below 35 N/m and adequate backside roller cooling are typical starting points to avoid local stretching. On cast film lines, the lower film crystallinity produced by rapid quenching influences slip additive migration and corona decay; tension control at the winder must accommodate the resulting coefficient-of-friction changes to avoid blocking and telescoped rolls.
Nominal physical property coordinates for `Sclair® 11J4` are summarized below. These values are representative from supplier technical literature and are not specification limits. The manufacturer’s certificate of analysis reports lot-specific melt index, density, and any agreed processability parameters.
| Property | Test method | Value | Unit |
|---|---|---|---|
| Nominal density | ASTM D1505 / ISO 1183-1 | 0.920 | g/cm³ |
| Melt index | ASTM D1238, 190 °C/2.16 kg | 1.0 | g/10 min |
| Vicat softening temperature | ASTM D1525 | 109 | °C |
| Melting peak temperature | ASTM D3418 | 123 | °C |
Regulatory applicability for converted film depends on the complete formulation, including masterbatch, printing ink, adhesive, and post-treatment. The following standards are typically referenced for polyethylene food-contact and industrial film structures.
| Regulation or standard | Relevant reference | Application condition |
|---|---|---|
| US FDA 21 CFR 177.1520 | Olefin polymers, including density and extraction limits | Direct food contact subject to end-use extraction limits and conditions of use |
| EU Regulation (EU) No 10/2011 | Plastic materials and articles in contact with food | Overall migration limit 10 mg/dm²; specific migration limits for additives and monomers apply |
| REACH Regulation (EC) No 1907/2006 | Article 6(3) polymer exemption | Polymer exempt from registration; imported monomer and additive substances require registration for the applicable tonnage band |
Pellet handling systems should be cleaned to avoid cross-contamination with polypropylene or HDPE fines. Polyethylene generally absorbs less than 0.01 wt% moisture at 23 °C and 50% RH, so pre-drying is not normally required. If bags are exposed to liquid water or condensation, drying at 80 °C for 2–4 h in a desiccant dryer removes surface moisture and reduces extrusion discontinuities. In bulk railcar unloading, transition times with other polyethylene grades can be minimized by purging dense-phase lines because pellet surface condition and pellet geometry may differ from HDPE blends. Long-term outdoor exposure of neat resin without ultraviolet stabilizer is not recommended; carbon black or HALS packages are required for multi-season agricultural service, and the resulting film must be validated under ASTM D4329 or equivalent weathering protocols.