| HS Code | 665638 |
| Density | 0.918 g/cm³ |
| Melt Index 190 C 2 16 Kg | 0.8 g/10 min |
| Melt Flow Ratio I21 I2 | 30 |
| Melting Point | 124 °C |
| Vicat Softening Point | 100 °C |
| Tensile Strength At Yield | 10.3 MPa |
| Tensile Strength At Break | 27.6 MPa |
| Elongation At Break | 800% |
| Flexural Modulus | 221 MPa |
| Dart Impact Strength | 120 g |
| Elmendorf Tear Strength Md | 300 g |
| Elmendorf Tear Strength Td | 500 g |
| Haze | 14% |
| Gloss 45 | 55% |
| Coefficient Of Friction | 0.2 |
| Low Temperature Brittleness | < -70 °C |
As an accredited NOVA Chemicals Sclair® 11J1 Octene LLDPE Film Resin factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | NOVA Chemicals Sclair® 11J1 Octene LLDPE Film Resin is supplied in 25 kg bags or 1,000 kg bulk bags. |
| Container Loading (20′ FCL) | 20′ FCL: 18 pallets, each with 55 x 25 kg bags; approximately 24.75 MT total, subject to container weight limits. |
| Shipping | NOVA Chemicals Sclair® 11J1 Octene LLDPE Film Resin is typically shipped as a non-hazardous polymer in 25 kg bags on stretch-wrapped pallets or in bulk trucks/railcars. It requires clean, dry transport, protected from moisture, heat, and contamination, with standard freight documentation and labeling. |
| Storage | Store NOVA Chemicals Sclair® 11J1 Octene LLDPE Film Resin in a cool, dry, well-ventilated indoor area, away from direct sunlight, heat, sparks, flames, and strong oxidizers. Keep original bags or containers closed, clean, and palletized off the floor. Protect from moisture, contamination, and prolonged UV exposure. Use proper grounding/bonding to prevent static discharge. Follow the manufacturer’s SDS and local regulations. |
| Shelf Life | Shelf life is typically two years from manufacture when stored unopened in a cool, dry, ventilated area away from direct sunlight. |
Blown-film extrusion of Sclair® 11J1 for heavy-duty industrial shipping sacks on three-layer high-output lines with internal bubble cooling typically places the octene-copolymer resin in the core at 55–65 wt%, a high-melt-strength LDPE at 20–30 wt% in the skin layers, and clean trim recycle at 10–15 wt%. The resin’s melt index of 1.0 g/10 min (ASTM D1238, 190 °C/2.16 kg) and density of 0.918 g/cm³ (ASTM D792) fall within the processing window for grooved-feed extruders of 30:1 L/D or greater, where feed-zone barrel temperatures are held at 175–185 °C and the adapter before the die is controlled at 205–225 °C to prevent gel formation from LDPE skins while maintaining LLDPE melt homogeneity. Die gap settings of 1.8–2.4 mm with a blow-up ratio of 2.2:1–2.8:1 and a frost line height of 6–8 die diameters allow sufficient transverse orientation without destabilizing the bubble at throughputs above 300 kg/h. Tear resistance in the final film is assessed according to ASTM D1922, puncture propagation according to ASTM D5748, and dart impact by ASTM D1709 Method A. Because the sacks are intended for non-food industrial cargo, compliance is governed by REACH Regulation (EC) No 1907/2006 Article 33 communication obligations rather than direct food-contact clearance. Gusseted sacks are drop-tested per ISO 7965-1 and cycle-load tested per ISO 7965-2, with terminal products including petrochemical shipping sacks, fertilizer bags, and compressed insulation packaging.
Silage covers and greenhouse cladding produced from Sclair® 11J1 exploit the C8 branch length to resist crack propagation at low temperatures after prolonged UV exposure. The tubular film is run on conventional blown-film towers with die gaps of 1.8–2.3 mm and blow-up ratios of 2.0:1–3.0:1; the resin is diluted with 20–30 wt% LDPE to stiffen bubble geometry and with 3–5 wt% of a UV-stabilizer masterbatch containing hindered amine light stabilizers and a triazine UV absorber, yielding a final HALS concentration of 0.06–0.12 wt% in the film. Outdoor failure for silage covers is more closely correlated with tear propagation after surface pitting than with initial tensile yield; therefore quality control relies on ASTM D1922 Elmendorf tear and ASTM D5748 puncture retention after accelerated weatherability exposure per ISO 4892-3 Method A, cycle 2, with UV irradiance maintained at 0.50 W/m² at 340 nm. Melt temperatures at the die lip are kept below 215 °C to reduce oxidative degradation of the stabilizer package; the resin is not pre-dried unless silo storage has raised moisture above 0.05 wt%, an uncommon condition for polyethylene. For non-food agricultural film, REACH (EC) No 1907/2006 remains the principal regulatory framework, and the final article must not contain substances in Annex XVII beyond the stated restrictions. Terminal products include anaerobic silage barrier covers, tunnel greenhouse sheeting, and temporary fumigation liners.
On high-speed cast lines running pallet stretch film at 300–600 m/min, Sclair® 11J1 is introduced as a core-layer or intermediate-layer component in ABA coextrusion because its 1.0 g/10 min melt index and 0.918 g/cm³ density reduce melt curtain sag while retaining enough melt strength to limit neck-in across an air gap of 15–30 cm. A quantitative formulation for an AB structure consists of 20–30 wt% Sclair® 11J1 in the core, 60–70 wt% metallocene-catalyzed ethylene-octene plastomer with density 0.912 g/cm³ in the cling layer, and 1.5–2.5 wt% polyisobutylene-based tackifier masterbatch or a low-density cling additive in the cling layer only. When the resin is processed through a three-extruder cast line with screw diameters of 75–120 mm, L/D of 30:1 or greater, and die gaps of 0.6–0.9 mm, the melt temperature is set at 240–250 °C to minimize melt fracture, while the chill roll temperature is held at 18–24 °C to freeze the desired cling surface. Neck-in is measured directly at the die edge with an infrared camera and is typically specified as a percentage of die width; operators adjust the air gap and die lip heater profile rather than resin ratio to maintain neck-in below the design limit. Cling force is quantified according to ASTM D5458, and film puncture resistance is tested with ASTM D5748. Industrial non-food stretch wrap falls under REACH (EC) No 1907/2006; food wrap extensions require additional migration testing under EU No 10/2011 if the film contacts fatty foods. Terminal products include machine pallet wrapping and bundling film for cold-chain logistics.
Three-layer coextrusion lines for frozen food packaging position Sclair® 11J1 in the sealant layer or core to use the octene-branch distribution for low-temperature impact resistance at -40 °C, as measured by ASTM D3420 pendulum impact and ASTM D1922 tear. A typical sealant-layer formulation contains 85 wt% Sclair® 11J1, 10 wt% LDPE with a melt index of 2.0 g/10 min, and 5 wt% polymer processing aid masterbatch based on a fluoroelastomer at 2 wt% active content to suppress melt fracture on the die lip. The blown-film die is equipped with a dual-lip air ring and internal bubble cooling, with a die gap of 2.0 mm, a blow-up ratio of 2.5:1, and a frost line height of 5–8 die diameters. Seal initiation is evaluated according to ASTM F88 with a dwell time of 0.5 s and sealing pressure of 0.275 MPa.
| Regulation / Standard | Designation | Required Condition for Final Article |
|---|---|---|
| US FDA olefin polymers | 21 CFR 177.1520(c) 3.1a | Food-contact use under conditions A–H after final migration testing |
| EU plastics regulation | EU No 10/2011 Annex I | Overall migration ≤ 10 mg/dm² for simulant assigned by Annex III |
| REACH | EC No 1907/2006 Article 33 | SVHC communication in supply chain |
Terminal products include frozen vegetable pouches, ice cream overwrap, and marinated meat bags that must survive high-speed vertical form-fill-seal equipment running at 60–100 cycles/min. The sealant layer is not pre-dried unless storage relative humidity exceeds 60%; if pre-drying is applied, it is limited to 60–70 °C for 2 h in dehumidified hopper dryers to avoid additive bloom. Published data for this specific multilayer configuration is limited; migration testing on the final structure is therefore mandatory before food-contact release.
In extrusion lamination of PET or BOPP to aluminum foil, Sclair® 11J1 is substituted for a portion of conventional LDPE in the sealant web to raise hot-tack and puncture performance without shifting the neck-in profile beyond acceptable limits. The coextrusion lamination process uses a primary extruder delivering 50 wt% LDPE at 320–330 °C and a secondary extruder delivering 50 wt% Sclair® 11J1 at 300–315 °C, with a flat die gap of 0.4–0.8 mm and a line speed of 150–250 m/min. The two-layer melt curtain is drawn into a nip against a chill roll at 15–20 °C; melt web neck-in is measured according to internal QC, with the Sclair® 11J1-containing layer placed away from the substrate to preserve adhesion. Heat seal strength is tested per ASTM F88, hot-tack according to ASTM F1921, and coefficient of friction per ISO 8295. Because lamination sealant layers can contact dry foods, the structure is subject to FDA 21 CFR 177.1520 and EU No 10/2011; residual solvent and lamination adhesive are evaluated separately under EU No 10/2011 Article 3 and 21 CFR 175.105 for the adhesive component. Terminal products include lidding films for dry-mix pouches, laminated coffee bags, and metallized barrier sachets.
Extruded can liners and heavy refuse sacks based on Sclair® 11J1 are processed on low-inventory tubular lines where melt temperature control is more difficult than on high-output IBC systems. The formulation consists of 70–85 wt% Sclair® 11J1, 10–25 wt% post-industrial reclaim, and 3–5 wt% of a combined slip/antiblock masterbatch with erucamide at 5000 ppm active concentration and synthetic silica at 10,000 ppm to keep film-to-film friction below a static coefficient of 0.25 as measured by ISO 8295. The die gap is widened to 2.2–2.6 mm to compensate for lower draw-down capability in comparison with metallocene grades, and blow-up ratios are limited to 2.0:1–2.5:1 to prevent film splitting at the frost line when the ambient plant temperature falls below 15 °C. Puncture retention after stretching is characterized by ASTM D5748, and the material’s high molecular weight fraction contributes to lower gel counts after reclaim addition if the reclaim is melt-filtered through a 100-mesh screen pack. Because can liners are non-food and single-use industrial articles, regulatory compliance is limited to REACH (EC) No 1907/2006 and the absence of Annex XVII restricted substances. Terminal products include 208-litre drum liners, refuse sacks, and medical waste collection bags for low-temperature transport where the film must survive filling stresses and low-temperature impact.
Competitive NOVA Chemicals Sclair® 11J1 Octene LLDPE Film Resin prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Designated under the trade name Sclair 11J1, this linear low-density polyethylene is a 1-octene copolymer supplied by NOVA Chemicals for blown-film and cast-film conversion. The grade is specified with a nominal melt index of 1.0 g/10 min measured under ASTM D1238 at 190 °C with a 2.16 kg load, and with a nominal solid-phase density of 0.918 g/cm³ measured under ASTM D792. By incorporating 1-octene rather than 1-butene as comonomer, the resin carries C8 short-chain branches along the ethylene backbone. That molecular feature changes crystallisation behaviour and mechanical failure mode in the finished film. The product is therefore positioned in applications where downgauging, puncture resistance, and orientation-induced tear resistance are process-critical: heavy-duty sacks, industrial liners, agricultural silage and greenhouse film, collation shrink, and sealant webs in food packaging. Because the grade is a linear polymer, its shear and extensional rheology differ from conventional LDPE on the same extrusion line, and the converter may need to adjust die gap, temperature profile, and air-ring settings to maintain stable bubble geometry.
The C8 comonomer influences failure resistance through lamellar thickness distribution and tie-molecule probability. At equivalent comonomer molar content and equivalent crystallinity, a longer branch is more efficient at interrupting crystalline order, and tie-molecule concentration is generally higher. The resulting film converts impact energy into plastic yielding rather than crack propagation, raising the force required for tearing and puncture. Comparative blown-film evaluations intended to isolate the comonomer effect often use a melt index of 1.0 g/10 min and a density of 0.918 g/cm³, matching the Sclair 11J1 specification. Under ASTM D1709, Method A, published comparative data for C8-LLDPE films of this density class commonly show dart impact improvements of 20% to 50% relative to C4-LLDPE at equal gauge, although line-specific variation may exceed that range. Under ASTM D1922, transverse-direction Elmendorf tear is typically the most sensitive property because machine-direction orientation generated during bubble stretching and collapsing suppresses machine-direction tear differences.
At a crystallinity of approximately 45% to 50%, film produced from Sclair 11J1 balances stiffness and flexibility. Tensile properties obtained under ASTM D882 typically show elongations at break above 600% for many blown-film conditions. Puncture resistance measured under ASTM D5748 is controlled by the same tie-molecule and orientation balance; agricultural hauling and aggregate-filled sacks require sufficient puncture resistance to avoid pinholing. Seal properties measured by ASTM F88 benefit from the lower melting peak associated with octene comonomer distribution. The seal-initiation temperature is not a single material parameter because it depends on dwell time, jaw pressure, and film gauge. On a rotary hot-bar sealing line, a reduction of 5 °C to 10 °C in jaw temperature relative to LDPE is often obtainable, but production validation should record actual seal strength and failure mode under ASTM F88.
Blown-film conversion of Sclair 11J1 is typically performed with melt temperature between 190 °C and 230 °C, a die gap between 1.5 mm and 2.5 mm, and a blow-up ratio between 2.0 and 3.0. Linear LLDPE develops higher shear viscosity than LDPE at equivalent melt index, so extruder motor load, melt pressure, and melt temperature rise are higher. A single-screw extruder with an L/D of 24:1 to 30:1, a barrier screw, and a spiral or Maddock mixer is recommended to complete melting without excessive shear heating. On a 65 mm extruder running at 100 rpm, die pressure can exceed 300 bar depending on die diameter, die gap, and temperature profile; comprehensive published data for this exact configuration is limited. Such pressure levels are normal for LLDPE but may overload an LDPE-configured machine with a low-torque drive or shallow melt channel.
Bubble stability of Sclair 11J1 is lower than LDPE because the linear chain extensional viscosity lacks long-chain branching. With a single-lip air ring, frost line height is commonly held below 800 mm for a 25 µm film to preserve transverse-direction tear. Internal bubble cooling or a dual-lip air ring is often used when specific output exceeds 10 kg/h/cm of die circumference. Sharkskin and die-lip melt fracture are managed with die-lip geometry and temperature; die gaps below 1.0 mm may increase die pressure without improving bubble stability. If gel accumulation appears, lowering adapter and die-body temperatures to 200 °C and reducing residence time is preferred. A short streamlined adapter and a spiral mandrel die with low surface roughness reduce degradation risk during extended runs.
A converter replacing a C4-LLDPE or LDPE at 25 µm thickness with Sclair 11J1 can generally expect improved downgauging potential. The octene resin commonly permits a thickness reduction of 15% to 25% while retaining equivalent dart impact and tear performance in heavy-duty packaging, but this is formulation- and line-specific and should be confirmed through statistical process capability studies. For heavy-duty sacks, a starting formulation of 70% Sclair 11J1 with 30% LDPE balances bubble stability, sealability, and stiffness. The LDPE phase increases extensional melt strength and widens the processing window but reduces tear and impact in proportion to LDPE content. Blending with C4-LLDPE at levels above 30% can reduce transverse-direction tear sharply. Because transverse-direction tear is a primary failure mode in loaded sacks, laboratory tear measurements under ASTM D1922 and field drop tests are required before and after any blend change. In coextruded structures, Sclair 11J1 can be used as the core or seal layer; the skin layer is often an LDPE or C4-LLDPE selected for seal and hot-tack properties measured under ASTM F1921.
| Property | Test method | C₄-LLDPE | C₈-LLDPE class | LDPE |
|---|---|---|---|---|
| Melt index | ASTM D1238 | 1.0 g/10 min | 1.0 g/10 min | 1.0 g/10 min |
| Density | ASTM D792 | 0.918 g/cm³ | 0.918 g/cm³ | 0.918 g/cm³ |
| Dart impact | ASTM D1709 | Lower | Higher | Lowest |
| Elmendorf tear, transverse direction | ASTM D1922 | Lower | Higher | Variable |
| Puncture resistance | ASTM D5748 | Lower | Higher | Lower |
| Melt strength | Extensional rheometry | Low | Low | High |
Food-contact structures using Sclair 11J1 as a sealant or core layer are evaluated under FDA 21 CFR 177.1520 in the United States and under Commission Regulation (EU) No 10/2011 in the European Union. The suitability for food contact depends on intended conditions of use, food simulant, contact time, and film thickness. Converters should obtain a food-contact statement from NOVA Chemicals for the specific grade and lot because additive packages, catalyst-neutralising agents, and external coatings can alter migration performance. A compliance checklist for film production typically includes density and melt index certificates under ASTM D792 and ASTM D1238, tensile data under ASTM D882, seal strength under ASTM F88, and coefficient of friction under ASTM D1894 when slip is present. For the European Union, overall migration testing is performed according to EN 1186, and specific migration according to EN 13130 when applicable.
| Parameter | Standard or regulation | Typical test condition |
|---|---|---|
| Melt flow rate | ASTM D1238 / ISO 1133-1 | 190 °C, 2.16 kg |
| Density | ASTM D792 / ISO 1183-1 | 23 °C |
| Tensile film | ASTM D882 / ISO 527-3 | 500 mm/min |
| Dart impact | ASTM D1709 | Method A, 26 in drop |
| Elmendorf tear | ASTM D1922 | Notched, 800 g pendulum |
| Heat seal strength | ASTM F88 | Seal and peel |
| Coefficient of friction | ASTM D1894 | Film-to-film |
| US food contact | FDA 21 CFR 177.1520 | Intended use |
| EU food contact | EU 10/2011 | Overall migration |
| REACH | Regulation (EC) 1907/2006 | Article registration |
Thermal degradation of Sclair 11J1 is minimised when melt temperature is kept below 240 °C and hold-up time is not prolonged. The stabilisation package protects the melt against oxidation during normal extrusion, but repeated regrind incorporation above 20% can shift melt index and increase gel formation. Film with high gel load may show reduced dart impact under ASTM D1709 and increased tear variability under ASTM D1922. When blending with a slip masterbatch, the converter should verify that erucamide or oleamide migration at room temperature does not saturate the surface and lower seal strength. Amine-containing additives are not generally incompatible with the grade, but acidic neutraliser residues from other resins can consume hindered amine light stabilizers during processing. In high-UV agricultural film, carbon black or a hindered amine light stabilizer package is necessary because unstabilised polyethylene loses elongation rapidly, as measured by ASTM D4329 or ASTM D638 after accelerated weathering.
Storage and handling of Sclair 11J1 are straightforward because polyethylene is non-hygroscopic. Pre-drying is not required unless surface condensation is present; if visible moisture is observed, warm-air drying at 60 °C for 1 h is sufficient. Pellets should be stored below 40 °C in a covered silo or supersack. Outdoor open storage should be limited to avoid UV surface oxidation and iron contamination from conveyor transfer. Cleanout and purging after processing require a material with sufficient viscosity; a fractional-melt HDPE purge resin or a 0.5 g/10 min LDPE is preferred to displace LLDPE from die lips and screen packs. The purge should be run at 200 °C to 220 °C until the melt appears homogeneous. After shutdown, the die should be starve-fed or filled with purge resin to reduce oxygen contact at hot metal surfaces. Screen-pack changes should follow extruder manufacturer safety instructions and be performed at process temperature to avoid melted polymer solidification in the breaker plate.