| HS Code | 906861 |
| Comonomer | Octene |
| Melt Index 190 C 2 16 Kg | 0.90 g/10 min |
| Density | 0.919 g/cm³ |
| Melting Point Dsc | 122 °C |
| Vicat Softening Point | 95 °C |
| Tensile Strength At Yield Md | 10 MPa |
| Tensile Strength At Yield Td | 10 MPa |
| Tensile Strength At Break Md | 34 MPa |
| Tensile Strength At Break Td | 31 MPa |
| Elongation At Break Md | 700% |
| Elongation At Break Td | 800% |
| Dart Drop Impact | 200 g |
| Elmendorf Tear Strength Md | 250 g |
| Elmendorf Tear Strength Td | 500 g |
| Haze | 12% |
| Gloss 45 | 60% |
| Coefficient Of Friction | 0.20 |
| Blocking | 50 g |
As an accredited NOVA Chemicals Sclair® 11B4 Octene LLDPE Film Resin factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | NOVA Chemicals Sclair® 11B4 Octene LLDPE Film Resin typically comes in 25 kg polyethylene bags, palletized for shipping and storage. |
| Container Loading (20′ FCL) | 20′ FCL dry container: NOVA Sclair 11B4 LLDPE film resin, 25 kg bags, palletized, shrink-wrapped, floor-loaded; approximately 18–20 MT net. |
| Shipping | NOVA Chemicals Sclair® 11B4 Octene LLDPE Film Resin typically ships as non-hazardous polyethylene pellets in moisture-barrier bags, bulk bags, or bulk rail/truck. Keep dry, away from heat and contamination. No DOT/IMDG/IATA hazard classification; use standard handling. Consult SDS and shipping documents for packaging and transport details. |
| Storage | Store NOVA Chemicals Sclair® 11B4 Octene LLDPE Film Resin in a cool, dry, well-ventilated warehouse. Keep bags or containers sealed, palletized, and off the floor. Protect from direct sunlight, heat, moisture, and contamination. Avoid ignition sources, open flames, and strong odors. Use first-in, first-out rotation. Maintain clean handling areas and follow local storage and safety regulations. Keep away from incompatible materials. |
| Shelf Life | Shelf life is 24 months from date of manufacture when stored in original packaging in a clean, dry, covered area. |
At cast film line speeds above 450 m/min, the melt curtain formed from Sclair® 11B4 octene LLDPE is specified for pallet unitization where elongation at break and controlled unwind force are measured under ASTM D882 and ASTM D1894. The formulation is operated neat at 100 wt% Sclair® 11B4 for core and back layers of three-layer machine-wrap structures, or at 80–95 wt% when 5–20 wt% of a metallocene hexene LLDPE is added to the core layer to shift ASTM D1709 dart impact upward at equivalent gauge. Cling layers are dosed with 1–2 wt% polyisobutylene tackifier having number-average molecular weight in the 1,000–3,000 Da range, and a synthetic silica antiblock masterbatch is let down to 0.5–1.5 wt% in the skin layers to prevent blocking on the reel after winding at 30–45 N/cm tension. The conversion line is typically a single-screw extruder with 24:1 to 30:1 L/D and a barrier feed section, feeding a coextrusion feedblock connected to a flat die with a lip gap of 0.6–0.8 mm. Melt temperature is held at 255–265°C to keep the high-shear film bubble below the critical shear rate for sharkskin; at line speeds exceeding 450 m/min, lowering melt temperature below 245°C increases the probability of melt fracture at the die lip. The air gap is set at 100–150 mm, and chill-roll temperature is maintained at 18–22°C to generate a low-haze surface without quench-temperature cycling that lowers cling repeatability. On production cast film lines, neck-in is controlled by the combination of octene branch length, which reduces melt elasticity relative to LDPE, and the use of vacuum box or electrostatic pinning at the die lip; edge trim from the line can be recycled at 10–20 wt% into the core layer without exceeding a 0.2 dispersion gel level when a 100 µm screen pack is installed. End-product forms include 12–23 µm machine pallet wrap for automated turntable wrappers, 25–35 µm hand-applied pre-stretch film, and five-layer coextruded films in which Sclair® 11B4 serves as the tough back layer under a metallocene cling skin. Compliance for non-food industrial stretch film is assessed against EU Packaging Directive 94/62/EC Annex II heavy-metal limits, with lead, cadmium, mercury, and hexavalent chromium combined below 100 ppm, and against REACH Article 33 communication obligations for substances of very high concern. Peel cling is quantified under ASTM D5458, coefficient of friction under ASTM D1894, and elongation under ASTM D882. Published data for the specific Sclair® 11B4 coefficient-of-friction evolution after 14 days of aging on a finished reel is limited; converters should establish reel-to-reel variation on their own winders before setting automatic wrapper pre-stretch ratios above 250%.
| Standard or regulation | Measured attribute or compliance boundary | Application scenario |
|---|---|---|
| ASTM D1238 | Melt flow rate at 190°C/2.16 kg; incoming resin control | Cast film, blown film |
| ISO 1133-1:2022 | Melt flow rate for international specifications | Incoming resin control |
| ASTM D882 | Tensile and elongation at break | Cast film, blown film, air pillow film |
| ISO 527-3 | Tensile properties of film | Blown film, silage wrap |
| ASTM D1709 | Dart impact resistance | Heavy-duty sacks, blown film, frozen food structures |
| ISO 7765-1 | Dart impact resistance for thin film | Air pillow film, industrial film |
| ASTM D1894 | Coefficient of friction | Cling/antiblock evaluation |
| ASTM D5458 | Peel cling of stretch wrap | Machine wrap, hand pallet wrap |
| EN 14932:2006 | Thermoplastic stretch film for wrapping bales | Silage wrap |
| ISO 21898:2007 | Flexible intermediate bulk container performance | FIBC liners |
| FDA 21 CFR 177.1520(c) | Olefin polymer food-contact compliance | Frozen food, lamination sealant webs |
| EU Regulation (EC) No 10/2011 | Plastic food-contact overall migration limit 10 mg/dm² | Frozen food, lamination sealant webs |
| EU Packaging Directive 94/62/EC | Heavy-metal sum below 100 ppm | Industrial stretch wrap, heavy-duty sacks |
| EU Regulation (EC) No 2023/2006 | Good manufacturing practice for food-contact materials | Frozen food, lamination sealant webs |
| EU Regulation (EC) No 1907/2006 | REACH chemical restrictions and SVHC communication | All scenarios |
In frozen-food vertical form-fill-seal structures, the sealant web is produced from Sclair® 11B4 octene LLDPE where seal initiation temperature and low-temperature dart impact determine minimum package integrity at freezer distribution temperatures below -25°C. The formulation is set at 60–80 wt% Sclair® 11B4, with 10–25 wt% high-pressure LDPE having a melt flow rate of 0.25–0.5 dg/min for bubble stability and 10–15 wt% metallocene LLDPE for seal strengthening; a silica antiblock masterbatch is added at 0.5–1.5 wt%, and erucamide slip is adjusted to 500–1,500 ppm in the sealant skin. The web is blown on a three-layer coextrusion line at blow-up ratio 2.0–2.5:1, die gap 1.8–2.4 mm, and melt temperature 205–225°C; frost-line height is held at 6–10 die diameters to balance transverse-to-machine orientation. On vertical form-fill-seal equipment, the seal jaws operate at 110–125°C with dwell of 40–120 ms; the octene LLDPE sealant achieves a seal initiation range typical for the class at 90–110°C, though resin-specific verification against the supplier certificate of analysis is required. End-product formats include 40–80 µm pillow packs for frozen vegetables, pre-formed pouches for IQF shrimp, and side-gusseted bags for frozen ready-to-bake items. Food-contact compliance is controlled under FDA 21 CFR 177.1520(c) for olefin polymers and EU Regulation (EC) No 10/2011 with an overall migration limit of 10 mg/dm², supported by good manufacturing practice under EU Regulation (EC) No 2023/2006. Operational limits must be enforced: antiblock masterbatch above 2 wt% reduces low-temperature dart impact at -20°C, and erucamide above 1,500 ppm can bloom to the seal surface and lower seal strength by more than 15% after 72 h of aging. Published resin-specific low-temperature dart impact data for Sclair® 11B4 below 50 µm film are limited; converter trials on the target three-layer blown film line are required before final gauge reduction.
When a converter replaces a thicker LDPE sack structure with a downgauged Sclair® 11B4 film below 80 µm, the failure mode shifts from tensile yield to dart-impact puncture, and the formulation must compensate through blend design and bubble geometry. The formulation is compounded at 50–70 wt% Sclair® 11B4, 20–30 wt% post-industrial recycled LLDPE, 5–10 wt% LDPE for melt strength, and 2–4 wt% carbon black masterbatch; a fluoropolymer processing aid is added at 0.5–1.5 wt% to suppress die-lip buildup during multi-day runs. The film is blown on a monolayer or three-layer line at blow-up ratio 2.0–2.5:1, die gap 2.0–2.5 mm, and melt temperature 200–220°C. A screen pack combination with 74 µm opening is installed upstream of the die to remove carbon black agglomerates and recycled-material gels; agglomerates above 10 µm that survive filtration create pinholes when the film is drawn below 80 µm. End-product forms include FIBC liners tested under ISO 21898:2007, valve sacks for polymer granules, open-mouth sacks for resin pellet packaging, and heavy-duty liners for mineral powders. Compliance for packaging and packaging waste is referenced to EU Packaging Directive 94/62/EC Annex II heavy-metal limits, with the sum of lead, cadmium, mercury, and hexavalent chromium below 100 ppm. The main processing trade-off is that down-gauging below 80 µm shifts the failure mode from tensile yield to dart-impact puncture, so the line must operate at a lower frost-line height to preserve impact strength while avoiding excessive molecular orientation in the machine direction. Published data for the specific Sclair® 11B4 and post-industrial recycled blend is limited; each recycled source must be qualified by gel count and melt flow ratio before production.
Thin cast sealant webs for non-retort stand-up pouches use Sclair® 11B4 at 20–35 wt% in the sealant layer, blended with 65–80 wt% metallocene LLDPE, a silica antiblock masterbatch at 0.5–1.0 wt%, and erucamide slip at 500–1,000 ppm. The cast film is produced at die lip gap 0.5–0.7 mm, melt temperature 240–260°C, and chill-roll temperature 20–25°C, then adhesive-laminated to biaxially oriented PET, BOPP, or aluminium foil under nip loads of 50–80 N/cm. End-product types include dry-food stand-up pouches, coffee valve pouches, and rewind lamination webs for subsequent pouch conversion. Food-contact compliance follows FDA 21 CFR 177.1520(c), EU Regulation (EC) No 10/2011 with a 10 mg/dm² overall migration limit, and EU Regulation (EC) No 1935/2004; the converter must verify that the adhesive and printing system do not raise migration above the legal limit. Surface treatment to 38–42 mN/m is required before lamination; if treatment drops below 36 mN/m, peel adhesion at the secondary interface becomes discontinuous.
For round-bale silage wrap produced from Sclair® 11B4, UV stabilizer dosage and cling-layer repeatability are the controlling variables because the film survives multiple pre-stretch revolutions on the wrapper and continues to cling after outdoor exposure. The formulation is set at 70–90 wt% Sclair® 11B4, 10–30 wt% metallocene LLDPE for tack and puncture, 0.5–2.0 wt% HALS-based UV stabilizer masterbatch, 0.5–1.5 wt% cling agent, and 0.5–1.0 wt% antiblock masterbatch. The film is blown on a three-layer line at blow-up ratio 2.0–2.5:1, die gap 2.0–2.5 mm, and melt temperature 210–230°C; the resulting web is slit to 500 mm or 750 mm rolls for bale wrappers. During field operation, the pre-stretch unit is set at 55–70% elongation; lower pre-stretch leaves excessive residual stretch and higher pre-stretch above 70% can initiate cling-layer tearing on Sclair® 11B4-rich films. End-product forms include 25 µm round-bale silage wrap, haylage film for high-moisture forage, and black or white coextruded bale films for oxygen exclusion. Compliance is assessed under EN 14932:2006 for thermoplastic stretch films used for wrapping bales, with puncture and retention tests performed after accelerated UV aging; industrial chemical compliance follows REACH Annex XVII restrictions for substances in the final film. Addition of UV stabilizer masterbatch above 2.0 wt% raises coefficient of friction beyond the normal wrapper clutch limit, causing telescoping and inconsistent consecutive-bale wrapping. Published data for the specific Sclair® 11B4 UV aging profile at 12 months outdoor exposure is limited; field testing on wrapped bales must validate the final stabilizer package.
| Process configuration | Sclair® 11B4 proportion | Co-resin and additive proportion | Terminal product type |
|---|---|---|---|
| Cast stretch film | 80–100 wt% | 0–20 wt% metallocene LLDPE; 1–2 wt% polyisobutylene; 0.5–1.5 wt% antiblock | Machine wrap, hand pallet wrap |
| Frozen-food VFFS blown film | 60–80 wt% | 10–25 wt% LDPE; 10–15 wt% mLLDPE; 0.5–1.5 wt% antiblock; 500–1,500 ppm slip | Frozen vegetable pillow packs, IQF pouches |
| Heavy-duty sack film | 50–70 wt% | 20–30 wt% recycled LLDPE; 5–10 wt% LDPE; 2–4 wt% carbon black; 0.5–1.5 wt% processing aid | FIBC liners, valve sacks, open-mouth sacks |
| Lamination sealant web | 20–35 wt% | 65–80 wt% mLLDPE; 0.5–1.0 wt% antiblock; 500–1,000 ppm slip | Stand-up pouches, coffee valve pouches |
| Silage wrap blown film | 70–90 wt% | 10–30 wt% mLLDPE; 0.5–2.0 wt% UV stabilizer; 0.5–1.5 wt% cling agent | Round-bale silage wrap, haylage film |
| Air pillow cast film | 85–100 wt% | 0–15 wt% LDPE; 500–1,000 ppm slip; 0.2–1.0 wt% antistatic | Void-fill air pillows, cell cushioning |
At inflatable air pillow conversion, the film is cast at 25–30 µm from Sclair® 11B4 with a specific balance of low-temperature dart impact and controlled slip, because the post-conversion heat seal must not be compromised by surface bloom. The formulation uses 85–100 wt% Sclair® 11B4, 0–15 wt% LDPE for melt strength, erucamide slip at 500–1,000 ppm, and an antistatic masterbatch at 0.2–1.0 wt% to prevent dust attraction inside e-commerce cartons. The film is produced at die gap 0.5–0.7 mm, melt temperature 240–260°C, and chill-roll temperature 20–25°C, then slit to converter rolls for air pillow machines. Heat-seal stations on the inflatable packaging line operate at 120–160°C and form longitudinal channels that are inflated to 0.4–0.7 bar; the Sclair® 11B4-rich web retains channel integrity after repeated compression cycles. Terminal products include void-fill air pillows, interleaved cell cushioning, and inflatable liners for cold-chain shipments. Compliance is limited to non-food transport packaging and is evaluated under ASTM D882 for tensile properties and ISO 7765-1 for dart impact; the converter must verify that anti-static additive selection does not elevate surface resistivity above 1011 Ω/square if electronic goods are packed. Operational boundaries include avoiding slip-agent concentrations above 1,200 ppm, because excessive bloom can produce channel delamination at seal temperatures below 140°C.
Competitive NOVA Chemicals Sclair® 11B4 Octene LLDPE Film Resin prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Introduced as an octene linear low-density polyethylene film resin, NOVA Chemicals Sclair® 11B4 carries a nominal density of 0.919 g/cm³ when measured by ASTM D792 or ISO 1183-1, and a melt mass-flow rate of 0.75 g/10 min at 190°C/2.16 kg per ASTM D1238 or ISO 1133-1:2022. The resin is polymerized with 1-octene as comonomer; the comonomer introduces hexyl side branches that depress crystallite thickness and increase the concentration of stress-transmitting tie molecules relative to a butene-based LLDPE of equivalent density. The product is supplied in stabilized pellet form and is normally evaluated on blown-film lines before conversion into industrial packaging. Because the base grade does not define the final surface friction properties, the coefficient of friction and blocking response are governed by externally added slip and antiblock masterbatches and are tested under ASTM D1894 and ASTM D3354.
At equal density and melt index, Sclair® 11B4 differs from ethylene-butene copolymers in side-chain length: butene contributes ethyl branches, whereas 1-octene contributes hexyl branches. The longer pendant group alters interlamellar coupling because a hexyl branch extends farther into the amorphous interlayer and participates in a broader distribution of loop and tie chains. This molecular architecture tends to raise slow crack growth resistance measured by ASTM D1693 or ISO 16770, and it modifies tensile elongation at break measured under ASTM D882. Published side-by-side film data for this specific configuration may be limited; converters should therefore run comparative trials with the same die gap, bubble geometry, and frost-line height before substituting an octene grade into a formulation built around butene LLDPE. Direct replacement at identical melt temperature can shift dart impact values measured by ASTM D1709, and the resulting film may show a different machine-direction tear to transverse-direction tear balance measured by ASTM D1922. The higher comonomer content required for 0.919 g/cm³ density also lowers the peak melting point and may reduce heat-seal initiation temperature relative to a stiffer butene grade of equal density.
For heavy-duty shipping sacks, industrial liners, agricultural silage wrap, and freezer packaging, Sclair® 11B4 is typically processed on a 65 mm to 75 mm grooved-feed single-screw extruder with an L/D of 30:1, a barrier flight section, and a spiral mandrel die with a die gap between 1.4 mm and 2.0 mm. Blow-up ratio is generally maintained between 2.2 and 2.8, with frost line height adjusted to 500–800 mm depending on air-ring type. Under these conditions, web gauge variation on a 2.4 m annular die is commonly held within ±5% of target when measured by ASTM D374 Method C. Draw-down and stalk height must be controlled because the octene LLDPE strain-hardens less than high-pressure LDPE, and excessive stalk length may produce transverse-direction tear loss while raising bubble instability. A processing aid masterbatch is sometimes required on high-speed lines above 120 rpm screw speed if sharkskin melt fracture appears along die lips.
Seal initiation temperature of Sclair® 11B4 is typically lower than that of stiffer high-density polyethylene but higher than many high-clarity metallocene LLDPE grades when measured by ASTM F88 on 25 µm film; hot tack measured by ASTM F1921 is dependent on seal bar temperature and dwell time. On a 50 mm wide seal bar, a jaw pressure of 0.4 MPa and dwell time of 0.5 s are screening conditions; converters should map seal strength across 100–140°C because the actual seal plateau moves with coextruded skin layer composition and antiblock particle size.
Recommended melt temperature range is 200°C to 230°C for blown film and 220°C to 240°C for cast film. Sustained melt temperatures above 240°C accelerate oxidative chain scission and can raise gel particle count in film; below 190°C the higher molecular-weight tail may not fully plasticise, leading to visible melt streaks and surging on 65 mm extruders. Die body temperatures should be kept close to the melt temperature to avoid port-line hang-up. Pre-drying is normally unnecessary; if pellet surface condensation is present after outdoor storage, a 70°C pellet dryer for 2 h is adequate. The screw should provide moderate melt mixing without excessive shear heating; a single-flight barrier screw with a Maddock mixing section typically yields melt-temperature rise below 15°C across the screw at 100 rpm. Regrind addition of clean edge trim up to 30 wt% is common, but higher levels can reduce bubble stability and lower dart impact measured by ASTM D1709.
On a cast-film line with a 0.8 mm slit die and a 20°C polishing roll, the resin is typically extruded at 220–240°C; line speed is governed by draw resonance and edge-necking severity. Vacuum box extraction is normally used to stabilise the web edges, and edge trim levels above 20 wt% can increase gel flecks if trim is recycled without filtration. Melt pressure before the screen pack on a 65 mm extruder commonly remains below 35 MPa; a rapid pressure rise above this level indicates screen blockage or insufficient rear barrel temperatures.
Compared with high-pressure low-density polyethylene produced in autoclave or tubular reactors, Sclair® 11B4 is linear and contains no long-chain branching. This difference lowers melt strength and narrows the operating window for high-stalk extrusion; when high melt strength is required, converters commonly blend 5–15 wt% of a fractional-melt LDPE into the resin. Compared with metallocene-catalysed LLDPE, the octene Ziegler-Natta architecture of Sclair® 11B4 generally exhibits broader molecular-weight distribution, which improves extrusion back-pressure stability on older single-screw lines but may not match the dart impact of a narrow-composition mLLDPE at identical gauge. The choice between these resin families should be based on ASTM D1709, ASTM D1922, and ASTM D1003 haze data generated on the specific line, because die gap and air-ring turbulence alter relative rankings.
Film property data for Sclair® 11B4 should be generated only after specimens are conditioned at 23±2°C and 50±5% relative humidity for not less than 40 h per ASTM D1709. Tensile properties are measured at 500 mm/min jaw speed according to ASTM D882; tear values are measured by the Elmendorf method of ASTM D1922; haze is measured according to ASTM D1003 and gloss at 45° according to ASTM D2457. Because LLDPE is strain-rate sensitive, comparing a 25 µm film with a 50 µm film without thickness normalisation is invalid. Published datasheet values for this exact grade at 25 µm are available from NOVA Chemicals technical documentation; however, the draw-down ratio, die gap, and cooling rate on a specific blown-film tower produce enough orientation variation that in-house capability trials remain the determining dataset for product release.
The resin may be re-extruded as clean in-house trim; accumulation of antioxidant depletion and gel formation should be monitored by periodic melt index and film appearance testing. Storage should remain below 40°C and away from direct ultraviolet exposure, because ultraviolet irradiation depletes phenolic stabilizer and shifts the oxidation induction time measured by ASTM D3895 or ISO 11357-6. The resin is not recommended for prolonged exposure to strong oxidising agents at melt temperatures above 230°C. Spiral film structures containing nylon or EVOH barrier layers require tie resin selection based on peel adhesion testing according to ASTM F904; published data for this specific configuration is limited.
Environmental stress-crack resistance is relevant for packaging liquid or surfactant-containing products. The octene branch length and molecular-weight distribution increase resistance to slow crack growth; however, the specific ESCR value measured by ASTM D1693 is geometry-dependent. Compression moulded specimens must be notched under controlled depth and tested in a 50°C or 100°C bath with 10% Igepal CO-630 or a compatible surfactant; results are reported in hours and are not directly transferable to film service in aggressive hydrocarbons.
For food-contact packaging, the converter must verify that the finished structure, not only the raw resin, complies with the relevant national or regional migration limits. The matrix below summarises the core designations.
| Area | Reference standard or regulation | Condition or limit |
|---|---|---|
| U.S. food-contact olefin polymers | FDA 21 CFR 177.1520(c) | End-use extraction limits apply |
| EU plastic food-contact materials | Regulation (EU) No 10/2011 | Overall migration limit 10 mg/dm² per EN 1186 |
| Density | ASTM D792 / ISO 1183-1 | 23°C |
| Melt mass-flow rate | ASTM D1238 / ISO 1133-1 | 190°C/2.16 kg |
| Film dart impact | ASTM D1709 | Method A or B according to gauge |
| Film tear resistance | ASTM D1922 | Elmendorf specimen geometry |
The density and melt-flow rate test methods cited for the base resin are the primary release parameters; conformance to regulatory status should be confirmed by the supplier’s compliance statement for the specific lot because additive masterbatches, printing inks, and tie layers alter the final migration profile.