| HS Code | 973250 |
| Productname | NOVA Chemicals Novapol PF-Y821-D Butene LLDPE Film Resin |
| Polymertype | Linear Low Density Polyethylene (LLDPE) |
| Comonomer | Butene |
| Density | 0.920 g/cm³ |
| Meltindex | 0.8 g/10 min (190°C/2.16 kg) |
| Meltingpoint | 124 °C |
| Vicatsofteningpoint | 100 °C |
| Tensilestrengthatyieldmd | 1400 psi (9.65 MPa) |
| Tensilestrengthatyieldtd | 1400 psi (9.65 MPa) |
| Tensilestrengthatbreakmd | 4500 psi (31.0 MPa) |
| Tensilestrengthatbreaktd | 4000 psi (27.6 MPa) |
| Elongationatbreakmd | 600 % |
| Elongationatbreaktd | 700 % |
| Dartimpact | 120 g |
| Elmendorftearmd | 200 g |
| Elmendorfteartd | 400 g |
| Haze | 12 % |
| Gloss45 | 55 % |
| Coefficientoffriction | 0.2 |
| Blocking | 50 g |
| Filmthicknessattest | 1 mil |
As an accredited NOVA Chemicals Novapol® PF-Y821-D Butene LLDPE Film Resin factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | NOVA Chemicals Novapol® PF-Y821-D Butene LLDPE Film Resin supplied in 25 kg bags, 40 bags per pallet, totaling 1,000 kg. |
| Container Loading (20′ FCL) | 20′ FCL: 25 kg bags, 55 bags per pallet, 10 pallets; approximately 13.75 metric tons net, stretch-wrapped and secured. |
| Shipping | NOVA Chemicals Novapol® PF-Y821-D Butene LLDPE Film Resin is shipped as free-flowing pellets in 25-kg polyethylene bags or bulk bags, palletized, stretch-wrapped, and labeled. Transport in clean, dry trucks or containers. Protect from moisture, contamination, excessive heat, and direct sunlight. Not classified as dangerous goods; follow SDS and local regulations. |
| Storage | Store NOVA Chemicals Novapol® PF-Y821-D Butene LLDPE Film Resin in a cool, dry, well-ventilated warehouse using original, closed packaging. Protect from direct sunlight, heat, ignition sources, moisture, dust, and contaminants. Keep away from oxidizing agents. Avoid excessive stacking and prolonged UV exposure. Reseal partially used bags. Practice first-in, first-out rotation. Do not store outdoors. Follow the SDS and local regulations. |
| Shelf Life | Shelf life is typically 24 months when stored in original, unopened packaging in a cool, dry place, away from sunlight and moisture. |
Novapol® PF-Y821-D is a butene comonomer linear low-density polyethylene film resin with nominal values of 0.921 g/cm³ density and 0.80 dg/min melt index measured under ASTM D1238 (190°C/2.16 kg), and these values position the material in the blown film envelope for heavy-duty shipping sacks and industrial liners where tear resistance and gauge reduction determine unit cost. The butene architecture is associated with lower dart impact than hexene LLDPE at equivalent melt index, so converters commonly verify heavy-gauge film under ASTM D1709 Method B and machine-direction tear under ASTM D1922 before approving a gauge reduction. Regulatory compliance for the converted article typically requires conformity to EU Directive 94/62/EC on packaging and packaging waste, REACH Regulation (EC) No 1907/2006 for substance registration, and for sacks subjected to dangerous goods transport, performance certification under UN 5H4 is the responsibility of the converter because the resin alone is not a certified packaging. Formulation on monolayer heavy-gauge lines commonly uses 70–85 wt% PF-Y821-D compounded with 15–30 wt% high-pressure LDPE having melt index 0.25–0.45 dg/min to raise bubble stability; a polymer processing aid masterbatch at 200–500 ppm active fluoropolymer is applied when die lip deposit or sharkskin appears above 80 m/min line speed. The downstream process is a single-screw extruder with L/D 24:1–30:1, barrier screw and Maddock mixing section, feeding a spiral mandrel die with die gap 1.8–2.5 mm, blow-up ratio 2.0:1–3.0:1, and melt temperature 180–210°C; on a 75 mm extruder with L/D 30:1, raising the frost line beyond 4 die diameters without increasing the LDPE fraction to 25 wt% typically produces visible bubble oscillation and gauge bands. Terminal articles produced from this configuration include heavy-duty shipping sacks for resin pellets, granular fertilizers and construction aggregates, as well as flat and gusseted industrial liners with film thicknesses from 80 µm to 200 µm.
Blown film intended for direct food contact under freezing conditions uses PF-Y821-D either neat or with 10–20 wt% high-pressure LDPE to lower back pressure and reduce melt temperature variation. Compliance is anchored to FDA 21 CFR 177.1520(c) for olefin polymers intended for food contact and to EU Regulation (EU) No 10/2011 Annex I with overall migration testing under Article 11 and Article 12, using food simulants appropriate to frozen aqueous and fatty food types; for low-temperature applications, the absence of high-temperature migration conditions simplifies the declaration but the film must still satisfy mono/oligomer restrictions under Annex I Table 1. The addition ratio for slip and antiblock masterbatch is 1.5–3.0 wt%, with silica-based antiblock selected at the lower end for films below 40 µm to limit haze. Low-temperature seal verification uses ASTM F88 and hot tack uses ASTM F1921; because butene LLDPE tends to exhibit weaker hot tack than hexene grades at equivalent density, PF-Y821-D is often paired with a metallocene outer layer when high-speed frozen food packaging requires seal strengths above 15 N/25 mm. Downstream production is performed on three-layer coextrusion blown film lines with die gap 1.5–2.0 mm, blow-up ratio 2.5:1–3.5:1, frost line height held at 2–4 die diameters, and melt temperature 185–215°C; exceeding 230°C degrades the antioxidant package and generates oxidation byproducts that may affect organoleptic properties in frozen food. Terminal film structures range from 25 µm to 80 µm and are converted into IQF vegetable pouches, frozen seafood bags, frozen meat overwrap, and pillow packs for loose-frozen products that require low-temperature dart impact and seal integrity at -30°C.
In agricultural silage and greenhouse covering, PF-Y821-D is formulated in three-layer structures where the core layer carries the mechanical load and the skin layers contain ultraviolet stabilizers; typical core content is 40–60 wt% of the total film thickness, with 15–35 wt% metallocene LLDPE added to the core to raise dart impact and tear resistance under ASTM D1709 and ASTM D1922. Compliance for covering films is assessed against EN 13206:2017 for greenhouse and low tunnel cladding, and silage preservation films are evaluated under EN 13207:2018; REACH registration for all ingredients in the UV masterbatch must be maintained, and no restricted phthalate or SVHC above 0.1 wt% may be introduced by the converter’s masterbatch. The UV/HALS masterbatch addition ratio is 3–6 wt%, with the HALS loading adjusted according to the intended service life, and an IR absorber or diffuser may be added to greenhouse grades at 1–3 wt% when light transmission targets are specified by the grower. Ultraviolet stabilization is assessed by accelerated weathering under ISO 4892-2 or ASTM G154, with tensile elongation retention of 50% after a specified radiation dose as the common agricultural film specification; published data for PF-Y821-D in 36-month greenhouse applications is limited, so converter-specific weathering trials are required. Production uses three-layer blown film lines with die gap 1.8–2.4 mm, blow-up ratio 2.8:1–4.0:1, and melt temperature 190–215°C; the bubble is kept at a low frost line to preserve impact properties, but too low a frost line increases film blocking on the collapsed frame if the antiblock level in the skins is below 0.8 wt%. Finished products include greenhouse cladding film, low tunnel film, UVI-stabilized silage covers, and temporary agricultural construction film with service lives from 6 to 36 months depending on stabilizer concentration.
High-speed vertical form-fill-seal conversion of dry food and pet food packets imposes a narrow seal initiation window because dwell times below 100 ms require the sealant layer to develop hot tack before the filling load opens the seal. PF-Y821-D can be used as a 40–60 wt% skin or sealant layer in a three-layer blown structure, with the core containing HDPE or MDPE for stiffness and the outer layer containing a higher-slip LLDPE for mandrel release; in monoweb applications, the resin is used at 95–100 wt% with 1–2 wt% slip/antiblock masterbatch. Food-contact compliance is based on FDA 21 CFR 177.1520(c) and EU Regulation (EU) No 10/2011, with migration testing under Article 11; for dry non-fatty foods, test conditions of 10 days at 20°C or 10 days at 40°C may apply depending on the intended shelf-life labeling. Hot tack performance is measured under ASTM F1921 at 100–140°C seal bar temperature and 0.3–0.5 MPa jaw pressure; because dwell time on vertical FFS lines may be below 100 ms, the sealant layer is formulated at a thickness not less than 12 µm to provide sufficient melt volume for seal formation. Downstream processing uses blown film coextrusion with die gap 1.5–2.5 mm, blow-up ratio 2.0:1–2.8:1, and melt temperature 180–215°C; the sealant layer must be positioned on the inside of the bubble to minimize contamination with slip additives from the outer layer, otherwise seal strength measured by ASTM F88 can fall below 10 N/25 mm at high line speeds. Terminal pouch structures range from 40 µm to 90 µm and include rice and grain pouches, pet food bags, seasoning sachets, and dry beverage mix pouches made on vertical FFS machines operating at 40–90 m/min.
For retail carrier bags and institutional can liners, PF-Y821-D is commonly diluted with post-industrial recycled LLDPE/LDPE and small HDPE fractions to balance stiffness and tear resistance while controlling resin cost per metre of film. A typical formulation is 50–70 wt% PF-Y821-D, 20–40 wt% post-industrial recycled LLDPE, and 10–20 wt% high-stiffness HDPE, with a fluoropolymer processing aid at 200–400 ppm to control melt fracture on high-output lines. Regulatory compliance is defined by EU Directive 94/62/EC for packaging waste and REACH Regulation (EC) No 1907/2006 for recycled feedstock traceability; when the bags are used for municipal waste collection, the converter may also verify tear and tensile properties under ASTM D1922 and ASTM D882. Recycled content varies batch-to-batch in melt index and gel count, so converters use a 80–120 mesh screen pack and maintain back pressure below 35 MPa to avoid unmelted gels causing film splits. Processing is performed on high-output monolayer blown film lines with 1.0–1.6 mm die gap, 3.0:1–4.0:1 blow-up ratio, and melt temperature 185–210°C; output rates above 3 kg/h/mm die circumference require internal bubble cooling because the high frost line associated with HDPE-rich blends reduces bubble stability and creates edge gauging. Finished products include T-shirt grocery bags, swing bags, institutional can liners, and heavy-duty refuse sacks in thicknesses from 20 µm to 60 µm.
In dry-food and frozen-food laminates, PF-Y821-D is converted into a blown sealant web that is subsequently adhesive-laminated to BOPP, PET, or paper; the sealant web accounts for 15–30% of the total laminate thickness and is typically produced at 20–50 µm before lamination. The resin is used at 80–100 wt%, with 0–20 wt% high-pressure LDPE added to adjust neck-in and bubble stability when the sealant web is run at higher blow-up ratios, but the addition of LDPE above 20 wt% lowers low-temperature seal strength and is avoided for frozen seafood laminates. Compliance for the finished laminate is confirmed under FDA 21 CFR 177.1520(c) and EU Regulation (EU) No 10/2011, with the adhesive layer requiring separate approval under Article 14 for dual-use additives and migration testing performed on the final laminate rather than the sealant web alone. Downstream production involves blown film extrusion with die gap 1.5–2.0 mm, blow-up ratio 2.2:1–3.2:1, and melt temperature 185–215°C, followed by solventless adhesive lamination at 200–400 m/min; the sealant web’s coefficient of friction must be confirmed by ASTM D1894 before lamination because slip additive bloom can reduce adhesive wetting if the web is stored longer than 48 h at ambient temperature. A coefficient of friction below 0.4 on the sealant web before lamination may indicate excessive slip bloom, which reduces adhesive wetting; laminators therefore specify a maximum storage time of 48 h or corona re-treatment before adhesive application. Terminal laminate applications include dry soup mix pouches, snack food laminates, frozen item outer bags, and portion packs for powders that require a hermetic seal and puncture-resistant outer ply.
Competitive NOVA Chemicals Novapol® PF-Y821-D Butene LLDPE Film Resin prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Novapol® PF-Y821-D is a butene-comonomer linear low-density polyethylene film resin supplied by NOVA Chemicals and positioned for cast-film conversion. The grade is identified by a nominal density of 0.921 g/cm³ tested under ASTM D1505 and a nominal melt index of 1.0 g/10 min at 190°C/2.16 kg using ASTM D1238. The polymer backbone is produced with 1-butene as the short-chain branch source; this architecture suppresses crystallinity below that of high-density polyethylene but does not create the long-chain branching characteristic of high-pressure low-density polyethylene. The suffix “D” denotes a formulation variant within the PF-Y821 family and is associated with an additive package intended for thin-gauge film, rather than a shift in base comonomer type or broad molecular weight distribution.
Procurement and incoming inspection of PF-Y821-D are typically controlled by lot-to-lot melt-index and density tolerance bands of ±0.1 g/10 min and ±0.001 g/cm³, respectively. Because polyethylene is not hygroscopic, pre-drying is not required for normal pellet transport; however, condensation on cold pellets can introduce surface moisture when silo discharge occurs under high-humidity conditions. A dry-air purge at the hopper inlet and a feed-throat temperature below 50°C are sufficient to prevent bridging.
Cast-film processing of PF-Y821-D is stable across a conventional melt-temperature band, but the lower melt strength of linear polyethylene limits the usable edge trim and draw-resonance boundaries. A production-scale line equipped with a 90 mm single-screw extruder, a 30:1 L/D barrier screw, and a screen pack of 60/80/100 mesh typically runs barrel setpoints of 190–230°C, adapter and die setpoints of 230–250°C, and a filtered melt temperature of 210–250°C. At melt temperatures below 200°C, shear heating may be insufficient to erase pellet memory at high throughput, resulting in visible flow lines at the die lip. Above 260°C, oxidative degradation in stagnant die-lip regions generates gel particles that transfer to the polished chill roll as surface defects. The processing window is therefore bounded on the low side by molecular relaxation and on the high side by thermal-oxidative stability, not by a sharp loss of film impact properties.
| Parameter | Method or instrument | Value or range | Notes |
|---|---|---|---|
| Density | ASTM D1505 | 0.921 g/cm³ | Nominal supplier value; acceptance commonly ±0.001 g/cm³ |
| Melt index | ASTM D1238 | 1.0 g/10 min | Condition 190°C/2.16 kg; acceptance commonly ±0.1 g/10 min |
| Comonomer | Supplier documentation | 1-butene | Short-chain branch source |
| Additive package | Certificate of analysis | Slip/antiblock variant | Confirm plate-out and roll-release behavior |
| DSC peak melting point | ASTM D3418 | 121–124°C | Second heating cycle at 10°C/min |
| Vicat softening point | ASTM D1525, A50 | 98–102°C | Typical C4 LLDPE range |
| Extrusion melt temperature | Production cast-film line | 210–250°C | Upper stability boundary 260°C |
| Chill-roll temperature | Polished two-roll stack | 18–24°C | Adjust for gauge and release |
Film testing should be delayed for 48 h after extrusion to allow post-crystallization and additive migration to reach a stable state. Conditioning at 23°C and 50% RH in accordance with ASTM D618 or ISO 291 is required before measuring tensile properties under ASTM D882, Elmendorf tear under ASTM D1922, dart impact under ASTM D1709, haze under ASTM D1003, gloss under ASTM D2457, and coefficient of friction under ASTM D1894. In published data for comparable butene LLDPE cast films of 25 µm gauge, machine-direction tensile strength at break commonly falls between 30–45 MPa, transverse-direction tensile strength at break between 25–35 MPa, elongation at break between 500–750%, and Elmendorf tear between 250–500 g in the transverse direction. These ranges are class-level values; PF-Y821-D may differ according to additive concentration, extrusion temperature, and draw ratio. Grade-specific results should be taken from the supplier’s current certificate of analysis or a controlled converter trial.
Die configuration exerts a strong influence on PF-Y821-D processing stability. The linear chain structure produces lower die-lip swell than LDPE; therefore, the die gap must be set narrower than for an LDPE melt to control overall film thickness. A typical cast-film die with a 0.5 mm lip gap and an internal deckle yields stable webs when the draw ratio is maintained between 15:1 and 25:1; above 30:1, draw resonance often appears as cyclic variation in machine-direction gauge. Edge bead stretching and trim recycling at rates up to 20 wt% are generally tolerated if the regrind is free of degraded polymer, but the addition of regrind can shift the effective slip concentration because the additive package is diluted and partially consumed during the first heat history.
The short-chain branch length imparted by 1-butene is shorter than that imparted by 1-hexene or 1-octene. At constant density, shorter branches produce a crystalline network with fewer interlamellar tie molecules, which reduces the energy required to propagate dart impact failure and lowers transverse-direction tear resistance relative to hexene and octene LLDPE grades. This is a structural consequence of the butene architecture, not an extrusion defect. In cast film, machine-direction orientation shifts the tear anisotropy; MD tear values are commonly lower than transverse-direction values because the oriented crystallites align in the machine direction and create a preferred tear path. When a converter requires increased dart impact or tear resistance, blending PF-Y821-D with 10–20 wt% of a hexene or octene LLDPE can raise tie-molecule concentration, but the blend may also increase haze and alter the slip additive migration rate.
Because PF-Y821-D does not contain long-chain branching, its shear-thinning response is less pronounced than that of LDPE. On a capillary rheometer at 190°C, the apparent viscosity of a linear butene LLDPE at low shear rate is higher than that of a branched LDPE of similar melt index, but at high shear rate the linear resin drops below the LDPE curve. This viscosity crossover has a direct effect on die-lip swell and melt curtain stability in cast-film extrusion. The lower die-lip swell of PF-Y821-D relative to LDPE permits tighter lip gaps and more precise thickness control, but it also reduces the polymer’s ability to resist draw resonance at high line speeds. Draw resonance in a cast line is typically managed by maintaining the draw ratio below 30:1 and by using an air knife or electrostatic pinning to stabilize the web at the chill roll.
Substitution of PF-Y821-D for a hexene or octene LLDPE is not a simple drop-in because the weaker tie-molecule network becomes more visible as gauge is reduced. In a downgauged stretch wrapper, the loss in dart impact may be partially offset by increasing film gauge by 2–4 µm, but this removes part of the economic benefit. A better route is to modify the cast line rather than the resin: raising the chill-roll temperature from 18°C to 24°C reduces quench-induced internal stress, while increasing the die gap from 0.4 mm to 0.6 mm lowers molecular orientation in the machine direction. These changes preserve transverse tear and seal performance at equivalent gauge.
| Polymer class | Comonomer | Density range | Melt index range | Tie-molecule network | Draw resonance resistance | Optical haze |
|---|---|---|---|---|---|---|
| Butene LLDPE, PF-Y821-D class | 1-butene | 0.921 g/cm³ | 1.0 g/10 min | Moderate | Low | High clarity |
| Hexene LLDPE | 1-hexene | 0.918–0.922 g/cm³ | 0.8–1.2 g/10 min | Higher | Low | Comparable clarity |
| Octene LLDPE | 1-octene | 0.916–0.920 g/cm³ | 0.8–1.2 g/10 min | Highest | Low | Good clarity |
| LDPE | None | 0.917–0.922 g/cm³ | 0.8–1.0 g/10 min | Low | High | Higher haze |
Additive migration kinetics in PF-Y821-D follow typical polyolefin behavior; the slip agent migrates to the surface over hours to days and is influenced by film crystallinity, storage temperature, and the presence of EVA or metallocene blend partners. A freshly cast PF-Y821-D film usually shows higher coefficient of friction than an aged film. Converters measuring slip properties should therefore delay coefficient of friction testing for at least 24 h, and preferably 48 h, after extrusion. If PF-Y821-D is used in a lamination sealant layer, the slip additive can bloom to the interface and reduce lamination bond strength; corona treatment before lamination can offset this effect by increasing surface energy and providing oxidation sites.
Compared with metallocene-catalyzed butene LLDPE of equivalent density and melt index, PF-Y821-D typically has a broader molecular weight distribution and a broader short-chain branch distribution. The broader molecular weight distribution improves extrusion torque and melt pressure in conventional single-screw lines, but it can produce slightly higher haze and lower dart impact. Metallocene grades often provide superior organoleptics and lower extractables, but they may require more careful temperature profiling because of their higher melt elasticity and different slip-additive interaction. PF-Y821-D is therefore selected where a conventional Ziegler-Natta butene resin provides adequate mechanical performance and the converter prioritizes process robustness over ultimate optical or dart properties.
Plate-out is a known bottleneck when running high-slip cast-film LLDPE grades on polished chill rolls. The slip component in PF-Y821-D can volatilize at die temperatures above 250°C and deposit on the chill roll as a waxy film. This deposit reduces heat-transfer coefficient and produces non-uniform quench, which can appear as transverse haze bands. The phenomenon is managed by limiting die temperature to 230–245°C, cleaning the roll with a non-abrasive polyolefin-safe purging compound, and avoiding prolonged idle at temperature. Production lines that run PF-Y821-D after a blown-film grade often observe a transient increase in plate-out until the die and roll reach a steady thermal equilibrium.
In a cast stretch-film line running PF-Y821-D at 25 µm, web stability is governed by the chill-roll release and the electrostatic pinning force. If the slip level in the formulation is too high, the melt curtain may slide along the chill roll and produce transverse gauge bands. If the slip level is too low, the formed film can block on the roll core and generate unwind noise. The required charge level for electrostatic pinning is typically set between 5 kV and 15 kV depending on line speed, web thickness, and ambient humidity. At relative humidity above 60%, static decay becomes faster and the pinning force degrades, requiring a higher charge setting or an air-knife assist. These interactions are direct field observations from cast-film production, not merely bench-scale rheology results.
For food-contact applications, PF-Y821-D is a polyolefin whose base polymer is generally covered by 21 CFR 177.1520 when the finished article meets the applicable extractives and end-use conditions. Under EU Regulation 10/2011 as amended, LLDPE films must comply with overall migration limits of 10 mg/dm² or 60 mg/kg depending on the packaging configuration. Converters should obtain a specific letter of assurance from the supplier for PF-Y821-D, because the final compliance status also depends on blend partners, colorants, and lamination adhesives. The resin is not designed for medical implant or parenteral applications, and no statement of USP Class VI or ISO 10993 suitability should be inferred from film-grade data alone.
For a horizontal form-fill-seal line using PF-Y821-D as the sealant layer in a lamination with biaxially oriented polypropylene, the sealing response is measured by ASTM F2029 for seal strength and ASTM F1921 for hot tack. Published data for this specific configuration is limited; converters should perform jaw-seal trials at their own dwell time and pressure because seal initiation shifts with jaw geometry and substrate thermal diffusivity. A typical starting condition for a butene LLDPE sealant web of this density is a jaw temperature of 110–125°C, dwell of 0.3–0.6 s, and pressure of 1.0–2.0 bar. The operational boundary is determined less by the resin melting point than by the rate at which the seal bar transfers heat through the outer web to the PF-Y821-D layer; low thermal conductivity outer layers require higher setpoints or longer dwell. The resin should not be combined with aggressive peroxide masterbatches unless the converter verifies absence of pre-crosslinking and gel formation in the extruder.