| HS Code | 636298 |
| Comonomer | Butene-1 |
| Melt Index | 1.0 g/10 min |
| Density | 0.918 g/cm³ |
| Melting Point | 120 °C |
| Vicat Softening Point | 95 °C |
| Tensile Strength At Yield Md | 1400 psi |
| Tensile Strength At Break Md | 4500 psi |
| Tensile Strength At Break Td | 4000 psi |
| Elongation At Break Md | 600 % |
| Elongation At Break Td | 700 % |
| Dart Drop Impact | 150 g |
| Elmendorf Tear Strength Md | 300 g |
| Elmendorf Tear Strength Td | 400 g |
| Haze | 10 % |
| Gloss | 70 % |
As an accredited NOVA Chemicals Novapol® PF-0118-B Butene LLDPE Film Resin factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | NOVA Chemicals Novapol® PF-0118-B Butene LLDPE Film Resin is packaged in 25 kg polyethylene bags, 50 bags per pallet (1,250 kg). |
| Container Loading (20′ FCL) | 20′ FCL loaded with NOVA Chemicals Novapol® PF-0118-B Butene LLDPE Film Resin, 25 kg bags, palletized, approx. 18–22 MT net. |
| Shipping | Shipping Description: Non-hazardous butene LLDPE film resin pellets; not regulated for DOT/IMDG/IATA. Packaged in 25 kg bags or bulk containers, palletized and stretch-wrapped. Transport in clean, dry vehicles. Store away from heat, sunlight, moisture, and ignition sources. Follow SDS and local regulations. |
| Storage | Store Novapol® PF-0118-B Butene LLDPE Film Resin indoors in a cool, dry, well-ventilated area. Keep original bags or containers closed, palletized, and protected from moisture, direct sunlight, excessive heat, ignition sources, and contamination. Avoid overstacking or damaging packaging. Use first-in, first-out. Maintain good housekeeping, inspect containers regularly, and keep away from incompatible materials. Follow the manufacturer’s SDS and local regulations. |
| Shelf Life | Typically 24 months from manufacture when stored in a cool, dry, well-ventilated area in unopened packaging, away from direct sunlight. |
Novapol® PF-0118-B is a butene linear low-density polyethylene film resin with a nominal density of 0.918 g/cm³ measured under ASTM D792-20 and a nominal melt index of 1.0 g/10 min measured under ASTM D1238-23 at 190°C/2.16 kg. The resin has been specified in blown-film and extrusion-lamination operations where butene comonomer distribution controls bubble stability, tear retention, and seal initiation without the narrower processing window of higher-alpha-olefin LLDPE grades. The profiles below are restricted to downstream processes for which this density and melt-flow class is documented in converter specifications.
For direct food-contact blown film, PF-0118-B is governed by FDA 21 CFR 177.1520(c) 3.2a for olefin polymers and by Regulation (EU) No 10/2011 with an overall migration limit of 10 mg/dm² determined in food simulants assigned by Annex III. The resin is processed as the food-contact layer at 100 wt% or at 70–90 wt% with 10–30 wt% LDPE homopolymer having a melt index of 0.25–2.0 g/10 min to improve bubble stability at BUR 2.5:1–3.0:1. Barrier or skin-layer masterbatches must use a polyethylene carrier and comply with 21 CFR 177.1520(c) or Regulation (EU) No 10/2011; total non-polymeric additive loading is maintained below 5 wt% unless migration modelling demonstrates no exceedance of the applicable migration limit. Processing on a grooved-feed single-screw blown-film extruder with L/D 24:1–30:1, barrel profile 175–210°C, melt temperature 193–216°C, die diameter 200–350 mm, die gap 1.8–2.4 mm, and dual-lip air ring cooling is used for gauge ranges of 20–80 µm. The frost line is maintained at 450–750 mm when the die diameter is 200 mm and BUR is 2.5:1; frost line heights below 350 mm reduce machine-direction tear by more than 15% under ASTM D1922-23, while heights above 900 mm degrade dart impact under ASTM D1709-24. The seal initiation window on 25 µm film is 105–120°C using a laboratory heat sealer at 2.0 bar and 1.0 s dwell with peel strength measured by ASTM F88/F88M-21. Terminal products include bread bags, frozen vegetable pouches, produce rollstock, and institutional kitchen film. Slip migration in two-layer constructions can shift seal-to-peel force by 5–10% after 14 days storage at 40°C; a full migration study under Regulation (EU) No 10/2011 is required before changing gauge or masterbatch level.
| Jurisdiction / Standard | Compliance Parameter | Test Method / Designation | Applied Limit |
|---|---|---|---|
| FDA 21 CFR 177.1520(c) 3.2a | Olefin polymer identity and specification | ASTM D792-20, ASTM D1238-23 | No specific SML; olefin polymer specification applies |
| Regulation (EU) No 10/2011 | Overall migration into food simulants | EN 1186-1:2002 | 10 mg/dm² |
| REACH Regulation (EC) No 1907/2006 | Substances of very high concern declaration | Article 33 communication | 0.1% w/w per article |
Heavy-duty sack and liner formulations based on PF-0118-B are compounded with post-consumer recyclate at converter-defined ratios because the end-use packaging is non-food-contact and is assessed under REACH Regulation (EC) No 1907/2006 and ISO 14021:2016. The line structure places PF-0118-B at 100 wt% in both outer skin layers, while the core layer contains 40–60 wt% PCR with the remainder PF-0118-B, yielding an overall PCR fraction of 20–30 wt%. On a 75 mm grooved-feed extruder with L/D 30:1, output is held at 350–400 kg/h; before the screen changer, melt pressure shifts from 12–15 MPa at start-up to 18–22 MPa after 3 h because gel and mixed-polyethylene domains accumulate on 120/200/120 mesh screen packs. When overall PCR exceeds 35 wt%, bubble geometry degrades into draw resonance, with layflat width oscillation at ±5 mm on a 200 mm die at BUR 2.8:1, and internal bubble cooling is required above 300 kg/h to keep frost line height below 900 mm. Film gauge is 100–180 µm, die gap 2.0–2.5 mm, and terminal products are construction powder sacks, petrochemical resin bag liners, mineral wool compression packaging, and FIBC liners. Puncture and tear properties are monitored by ASTM D1709-24 and ASTM D1922-23; a 40 wt% overall PCR loading reduces dart impact retention below 70% and requires an upgraded continuous belt melt filtration unit to maintain stable gauge.
The rheological mismatch between PF-0118-B and sorted post-consumer film arises from oxidative chain scission in previous heat histories; recyclate domains lower zero-shear viscosity but raise gel concentration, creating a bimodal flow profile at the die lip. To prevent melt fracture on sack surfaces, the outer layers are maintained at 100 wt% PF-0118-B with melt temperature 193–216°C, while the core containing PCR is run at 185–205°C. Die-lip build-up is removed when melt pressure before the breaker plate exceeds 25 MPa or when the pressure drop across the screen pack exceeds 6–8 MPa. Continuous melt filtration is warranted above 30 wt% overall PCR; without it, pressure spikes of 3–5 MPa per gel accumulation event are observed on melt transducers. Sack liners for hygroscopic mineral fillers are tested for moisture vapour transmission rate under ASTM F1249-20 at 38°C and 90% RH, with accepted values between 2.0–4.0 g/(m²·day) for 100 µm film; this range is controlled by film gauge and PCR content rather than by resin density alone.
| Formulation Variant | PF-0118-B Loading | Overall PCR Loading | Melt Pressure Before Screen Changer | Layflat Width Deviation | Dart Impact Retention by ASTM D1709-24 |
|---|---|---|---|---|---|
| Virgin reference | 100 wt% | 0 wt% | 12–15 MPa | ±2 mm | 100% |
| Core-layer PCR | 80 wt% | 20 wt% | 15–18 MPa | ±3 mm | 90–95% |
| Core-layer PCR | 70 wt% | 30 wt% | 18–22 MPa | ±5 mm | 80–85% |
| High-recyclate trial | 60 wt% | 40 wt% | 25 MPa after 2 h | ±10 mm | below 70% |
On three-layer agricultural film lines, PF-0118-B is processed as a core and skin component in mulch and bunker silo cover film. The core layer comprises 60–80 wt% PF-0118-B and 20–40 wt% LDPE/LLDPE let-down, while the outer layers carry 55–70 wt% PF-0118-B plus 2–5 wt% HALS-based UV masterbatch and, for silage cover, 3–6 wt% carbon black masterbatch with a polyethylene carrier. The applicable product standard is EN 13207:2018, which requires tensile properties according to EN ISO 527-3:2018 and impact resistance according to ISO 7765-1:2012. The process uses a three-layer blown-film die of 250–400 mm diameter, die gap 1.8–2.2 mm, BUR 2.5:1–3.2:1, melt temperatures of 200–220°C, and film thickness of 100–150 µm for silage clamp covers and 30–80 µm for mulch film. Terminal products include bunker silo sheets, silage clamp covers, nursery ground mulch, and low-tunnel greenhouse side curtains. PF-0118-B as supplied is not formulated for multi-season ultraviolet exposure; without the addition of the HALS-based UV package, outdoor weathering beyond 6 months produces surface crazing and reduces tensile elongation by more than 50% under EN ISO 527-3:2018. When pellets are stored at relative humidity above 60%, condensation on cold pellets can generate bubble voids and surface pitting; a hopper drying step at 60–70°C for 2 h is applied before extrusion in such conditions.
Extrusion lamination sealant layers using PF-0118-B are applied at coating weights of 15–30 g/m² on tandem extrusion-coating lines with slot die widths of 1200–1600 mm, extruders of L/D 32:1, melt temperatures of 270–290°C, air gap 150–250 mm, line speeds of 150–250 m/min, and chill roll surface temperatures of 8–15°C. The resin is used at 100 wt% or blended with 15–30 wt% LDPE homopolymer having a melt index of 4–7 g/10 min to reduce neck-in and improve adhesion to oriented polyester and aluminium foil. Neck-in at 280°C and 300 m/min is typically 8–15 mm per side for the unblended resin, falling to 6–10 mm per side when 20 wt% LDPE homopolymer is incorporated. Food-contact laminates are evaluated under FDA 21 CFR 177.1520(c) 3.2a and Regulation (EU) No 10/2011 with an overall migration limit of 10 mg/dm²; seal strength is measured by ASTM F88/F88M-21 on a structure of 12 µm PET / 7 µm aluminium foil / 25 µm sealant. When the sealant coating weight is reduced below 25 µm, pinhole frequency under dark-room light table inspection increases from below 1/m² to 3–5/m² if melt temperature falls below 275°C or chill roll temperature exceeds 15°C. Terminal products are dry-food sachets, frozen-food laminations, and non-retort pouch sealant webs. This resin is not substantiated for retort or boil-in-bag structures requiring sustained exposure above 95°C; published data for this specific configuration is limited, and end-user seal performance must be confirmed under actual filling line dwell time and jaw temperature.
For institutional refuse sacks and can liners, PF-0118-B is compounded at 65–80 wt% PF-0118-B, 10–20 wt% LDPE reclaim, 10–15 wt% calcium carbonate masterbatch, and 2–4 wt% black masterbatch with a polyethylene carrier. The applicable standard is EN 13592:2017 for household refuse sacks, covering dimensions, seal strength, and puncture resistance; non-food packaging compliance also includes REACH Regulation (EC) No 1907/2006. Processing is run on a single-screw high-stalk blown-film line with L/D 24:1–28:1, die diameter 150–250 mm, die gap 1.2–1.8 mm, BUR 3.0:1–4.0:1, film gauge 15–40 µm, and melt temperature 185–205°C. Screen packs of 80/100/80 mesh protect the die lip from carbonate agglomerates, and pressure drop across the pack is maintained below 8 MPa. Calcium carbonate loading above 15 wt% reduces Elmendorf tear by ASTM D1922-23 to below 70% of the unfilled film and reduces dart impact by ASTM D1709-24 below the range required for wet-refuse service; the described filler range is therefore restricted to light institutional sacks and can liners. Terminal products include janitorial can liners, retail refuse sacks, and light industrial bin liners. Film gauge below 15 µm run at BUR above 4.0:1 develops transverse-direction weave instability in the collapsing frame; on 200 mm dies, output is derated by 10–15% when the gauge set point is reduced to 12 µm to avoid layflat fluctuation exceeding ±4 mm.
Collation shrink film based on PF-0118-B is compounded at 80–90 wt% with 10–20 wt% LDPE homopolymer with melt index 0.3–0.8 g/10 min and processed through double-bubble or triple-bubble blown-film orientation. Free shrink is measured under ASTM D2732-23 at 130°C; converter specifications typically require machine-direction free shrink of 55–70% and transverse-direction free shrink of 45–60% on 50 µm film. First-bubble extrusion uses a die gap of 1.0–1.6 mm, BUR 1.8:1–2.2:1, and melt temperature 190–205°C; the second-stage reheating zone is maintained at 115–130°C, with machine-direction draw ratios of 3.5:1–5.0:1 and transverse-direction blow ratios of 3.0:1–4.0:1. Finished film thickness is 50–100 µm for beverage can and bottle bundles. At machine-direction draw ratios above 5.5:1, thickness bands exceed ±8% and free shrink variation exceeds ±5 absolute percentage points under ASTM D2732-23. Terminal products include collation shrink sleeves for bottled water, carbonated beverage multipacks, and household goods bundle wrap. Compliance is defined by REACH Regulation (EC) No 1907/2006 and CONEG heavy-metals limits for packaging; direct food contact is not intended for this configuration.
Competitive NOVA Chemicals Novapol® PF-0118-B Butene LLDPE Film Resin prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Resin selection for thin-gauge polyethylene film frequently begins with three parameters: comonomer type, density, and melt mass-flow rate. NOVA Chemicals Novapol® PF-0118-B is a butene-based linear low-density polyethylene film resin supplied with a nominal density of 0.918 g/cm³ and a nominal melt mass-flow rate of 1.0 g/10 min at 190°C under 2.16 kg load. The suffix “-B” designates the formulated additive package rather than the base copolymer; suffix changes within the PF-0118 series should not be treated as direct substitutions because slip and antiblock loadings can shift static coefficient of friction, blocking force, and optical haze. The product is directed toward general-purpose blown and cast film applications where intermediate toughness, a broad heat-seal range, and controlled surface slip are required.
The resin parameters commonly certified on the certificate of analysis include density and melt flow rate. Film property values are not usually certified because they depend on extrusion equipment, die gap, blow-up ratio, frost-line position, and cooling rate. Table 1 lists nominal resin values and class-typical ranges for blown film of this LLDPE density and melt-flow class at 25 µm gauge. The ranges are drawn from general butene-LLDPE production experience and supplier literature for this density and melt-flow class; they are not lot-acceptance limits.
| Parameter | Nominal value or class-typical range | Test method |
|---|---|---|
| Melt mass-flow rate | 1.0 g/10 min at 190°C/2.16 kg | ASTM D1238, ISO 1133-1 |
| Density | 0.918 g/cm³ | ASTM D1505, ISO 1183-1 |
| Comonomer type | Butene | Infrared spectroscopy, supplier method |
| Additive package | Slip and antiblock, suffix-dependent | Supplier certificate of analysis |
| Tensile strength at break, machine direction, 25 µm film | 30-45 MPa | ASTM D882, ISO 527-3 |
| Dart drop impact, F50, 25 µm film | 90-130 g | ASTM D1709, ISO 7765-1 |
| Elmendorf tear strength, machine direction/transverse direction | 100-180 g / 350-450 g | ASTM D1922, ISO 6383-2 |
| Optical haze, 25 µm film | 8-15% | ASTM D1003, ISO 14782 |
The use of ASTM D882 for tensile film properties, ASTM D1709 for dart drop impact, and ASTM D1922 for Elmendorf tear permits comparison only when film thickness, blow-up ratio, and frost-line history are reported. For the same nominal density and melt flow rate, film produced on a high-stalk line with internal bubble cooling can shift tear values by more than 10% from values obtained on a low-stalk line. Interlaboratory comparisons without equipment descriptions are therefore unreliable.
On production-scale blown-film lines, the melt-temperature window for this melt-flow class is ordinarily 190-230°C. Lower setpoints increase melt strength and improve bubble stability, while higher setpoints reduce melt pressure and may improve optical response. Extruder barrel profiles for 50-70 mm grooved-feed machines with 24:1-30:1 L/D are typically set from 175-185°C at the feed zone to 210-225°C at the die. Melt pressure at normal output commonly falls between 300 bar and 450 bar with a die gap of 1.5-2.5 mm; sustained pressure above 500 bar indicates screen-pack blinding, die-lip buildup, or excessive output for the die diameter. Polyethylene requires no drying at moisture levels below 0.05%, but condensation on cold pellets transferred into humid air can introduce surface defects. If condensation occurs, pellets should be held at 60-70°C for 2 h before feeding. Melt temperatures above 270°C are not recommended because oxidative degradation can produce gels, off-odor, and discoloration. Fluoropolymer processing aids are sometimes required at addition levels of 200-1000 ppm to suppress sharkskin melt fracture when die-lip shear stress exceeds the critical value; the exact threshold depends on die gap and melt temperature.
Die gap selection interacts directly with shear rate at the die lip. Narrow gaps below 1.0 mm increase shear rate and can initiate sharkskin on LLDPE. Wider gaps from 1.5 mm to 2.5 mm reduce die pressure and melt fracture but increase gauge-control demands. In coextruded structures, PF-0118-B is commonly placed in a skin or sub-skin layer to exploit slip and antiblock additive bloom. Erucamide-based slip additives migrate to the film surface over 24-72 h after extrusion; coefficient of friction measured by ASTM D1894 therefore decreases with time, and blocking force measured by ASTM D3354 can show the inverse trend if antiblock concentration is insufficient. Converters should avoid rapid stacking of warm slit rolls before the bloom period is complete because transient blocking can occur even when final coefficient of friction is within specification. Inorganic antiblock particles also influence optical haze and slitting-blade wear; published line data for this specific suffix is limited.
Food-contact status is not an intrinsic resin property; it is a function of the finished article, additive composition, and conversion conditions. For the United States, olefin polymers such as this butene LLDPE may fall under FDA 21 CFR 177.1520(c) when used in accordance with the use conditions and specifications of that section. Converters must verify whether the article is subject to 21 CFR 176.170(c) or other applicable provisions. For the European Union, the finished plastic material must comply with Commission Regulation (EU) No 10/2011, including the overall migration limit of 10 mg/dm² and any specific migration limits for monomers and additives. The polymer itself is normally exempt from registration under REACH Regulation (EC) No 1907/2006 as a polymer under Article 2(9), but the monomer and imported additives are subject to registration requirements. Table 2 summarizes the principal regulatory frameworks that may apply.
| Jurisdiction | Application area | Relevant clause or limit |
|---|---|---|
| United States | Food-contact olefin polymers | FDA 21 CFR 177.1520(c) |
| European Union | Plastic food-contact materials | Regulation (EU) No 10/2011, overall migration limit 10 mg/dm² |
| European Union | Chemical registration | REACH (EC) No 1907/2006, Article 2(9) polymer exemption |
| European Union | Restriction of hazardous substances in electrical and electronic equipment | Directive 2011/65/EU, 0.1% by weight for lead, mercury, hexavalent chromium, PBB, PBDE; 0.01% for cadmium |
The performance difference between butene, hexene, and octene LLDPE is dominated by short-chain branch length. Butene introduces ethyl branches, hexene introduces butyl branches, and octene introduces hexyl branches. At equivalent density and melt flow rate, longer branches create more effective disruption of lamellar thickness and a higher probability of tie-molecule formation. Hexene and octene LLDPE therefore generally provide higher dart drop impact, higher Elmendorf tear, and higher puncture resistance than butene LLDPE. A converter replacing PF-0118-B with a hexene or octene resin at the same density and melt flow rate may observe a measurable increase in toughness, but the magnitude cannot be predicted solely from density and melt flow rate; line trials should include ASTM D1709 dart impact, ASTM D1922 tear, and ASTM D5748 puncture tests.
Compared with low-density polyethylene, PF-0118-B has a linear backbone and lacks the long-chain branching of LDPE. As a result, it exhibits lower melt elasticity and lower bubble stability at high blow-up ratios, but it offers superior tensile elongation, dart impact, and seal strength at equivalent film gauge. Blending with 10-30% LDPE by mass is common to recover bubble stability; the exact ratio is set by die diameter, blow-up ratio, and output. Compared with metallocene LLDPE, conventional butene LLDPE has a broader molecular weight distribution and composition distribution. The broader distribution generally lowers melt pressure and improves extrusion stability but yields lower dart impact and higher extractables. Metallocene LLDPE may provide lower haze and higher toughness, but often requires tighter processing control and higher melt pressure.
PF-0118-B is typically considered for general-purpose film structures such as industrial liners, trash can liners, garment bags, laundry bags, overwrap, and agricultural films in gauges between 20 µm and 150 µm. It is not optimized for heavy-duty sack film requiring high puncture propagation resistance at sub-zero temperatures, nor for high-clarity shrink film where metallocene or LDPE-rich structures are preferred. For converter qualification, a design of experiments across die gap, blow-up ratio, frost-line height, and melt temperature is required; the resulting film should be tested under ASTM F88/F88M for seal strength, ASTM D1709 for dart impact, and ASTM D1922 for tear before release. Because lot-to-lot variation in slip additive bloom can affect downstream converting operations, incoming inspection should include coefficient of friction per ASTM D1894 after a standardized aging period of 48 h at 23°C and 50% relative humidity.