| HS Code | 294276 |
| Polymer Type | Polybutylene terephthalate (PBT) |
| Reinforcement | Glass fiber |
| Color | Black |
| Ul94 Rating | V-0 |
| Flame Retardant | Yes |
| Mold Shrinkage Percent | 0.2-0.5 |
| Volume Resistivity Ohm Cm | 1E15 |
As an accredited Nan Ya PBT-FR 1403G6 GBK4 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Nan Ya PBT-FR 1403G6 GBK4 is packed in 25 kg moisture-barrier bags, 40 bags per pallet (1,000 kg). |
| Container Loading (20′ FCL) | Loading Nan Ya PBT-FR 1403G6 GBK4 chemical into a 20-foot FCL container, ensuring secure, palletized stowage for safe transport. |
| Shipping | NAN YA PBT-FR 1403G6 GBK4 ships as black, glass-fiber-reinforced, flame-retardant PBT resin pellets in dry, sealed bags or containers. Normally non-hazardous and not regulated for transport; confirm against the current SDS. Protect from moisture, heat, and ignition sources; handle per supplier instructions. |
| Storage | Store Nan Ya PBT-FR 1403G6 GBK4 in a cool, dry, well-ventilated area, away from direct sunlight, heat, flames, and ignition sources. Keep original containers sealed and protected from moisture, dust, acids, alkalis, and strong oxidizers. Avoid crushing or prolonged stacking. Label clearly, use first-in/first-out, and follow the safety data sheet and local regulations. |
| Shelf Life | Typical shelf life is 12 months in original unopened packaging, stored dry and below 30°C. |
Competitive Nan Ya PBT-FR 1403G6 GBK4 prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Nan Ya PBT-FR 1403G6 GBK4 is a flame-retardant, 30 wt% glass fibre reinforced polybutylene terephthalate injection moulding compound supplied in black. The designation separates into PBT as the base resin, FR as the flame-retardant package, 1403G6 as the glass fibre and flow-modification series, and GBK4 as the black colour code. The compound is intended for electrical and electronic housings, connectors, relay bases, terminal blocks, and under-hood power distribution components where UL 94 V-0 classification, dimensional stability, and high stiffness are required. The product is normally processed by injection moulding; it is not optimised for extrusion or blow moulding because glass-fibre orientation distribution and flame-retardant thermal sensitivity differ from those processes. Processing and end-use decision-making should therefore begin with the lot-specific certificate rather than a generic PBT datasheet.
In PBT, rapid crystallisation from the melt produces a semi-crystalline matrix whose spherulite size is strongly affected by mould temperature. At a mould temperature below 60°C, the cooling rate suppresses full crystallinity and increases differential shrinkage between the oriented skin and core layers; at above 90°C, cycle time increases but post-mould shrinkage decreases. The 30 wt% glass fibre in PBT-FR 1403G6 GBK4 raises flexural modulus above 9,000 MPa and lowers mould shrinkage to approximately 0.2–0.6% in the flow direction, while transverse shrinkage can be 0.7–1.2% under ISO 294-4:2018. Warpage in thin-wall connectors is controlled by gate position and glass-fibre orientation; unbalanced gating produces differential orientation that cannot be corrected by mould temperature alone. Differential scanning calorimetry of PBT grades in this family typically shows a melting peak near 223–225°C under ISO 11357-3:2018, with crystallisation temperature near 190°C. The presence of the flame-retardant system shifts melt rheology relative to unfilled PBT, and the glass fibre contributes anisotropic shrinkage that must be reflected in tool compensation.
Before moulding, the pellets must be dried to a residual moisture content below 0.02% measured by ISO 15512:2022 method B. A desiccant dryer with a dew point of −30°C or lower and an inlet air temperature of 120–140°C for 3–4 h is the minimum practical configuration. Hydrolysis of the ester linkages in PBT is autocatalytic; at residual moisture above 0.05%, melt viscosity decreases and moulded parts exhibit surface silver streaks, reduced tensile strength, and embrittlement after thermal ageing. Hopper residence time at elevated temperature should not exceed 8 h because flame-retardant additives can migrate or degrade under prolonged hot-air exposure. Vacuum drying at 100°C may not remove moisture rapidly enough for high-volume production because the diffusion path through glass-filled pellets is longer than in unfilled resin.
Flame-retardant PBT compounds require a narrower processing window than non-FR grades. The melt temperature measured at the nozzle should be maintained between 245°C and 270°C. Above 280°C, brominated flame-retardant degradation accelerates, releasing acidic decomposition products that corrode screw and hot-runner surfaces and produce brown streaks. Residence time at melt temperature should be kept below 8 min; if the hot-runner volume exceeds two to three shot capacities, thermal stratification and black specks are observed in production. A three-zone screw with an L/D ratio of 20:1 to 24:1 and a compression ratio of 2.5:1 to 3.0:1 is appropriate. Back pressure should be set at 0.3–0.7 MPa hydraulic to homogenise the melt without excessive fibre attrition. Screw peripheral speed should remain near 5–10 m/min. Excessively high screw speed reduces average glass-fibre length from nominally 0.3 mm to below 0.2 mm and lowers tensile strength by 10–15%. Mould temperatures of 60–100°C are used; below 60°C the flame-retardant compound fills less predictably in thin ribs, and above 100°C cycle time increases without significant mechanical benefit. Published data for this specific configuration is limited for microcellular foaming and gas-assisted moulding; standard solid injection moulding is recommended.
The GBK4 black colour code identifies a carbon black-containing formulation. Carbon black can reduce surface resistivity slightly but is not sufficient to create an electrically conductive grade; volume resistivity typically remains above 1.0 × 1013 Ω·cm by IEC 62631-3-1. The black variant may show a 2–4% lower tensile strength than an uncoloured analogue because carbon black aggregates act as stress concentrators, and melt flow may differ by 1–2 cm3/10 min under the same ISO 1133-1:2022 conditions. Laser marking contrast of black GBK4 is limited; pad printing or label engraving is required for high-contrast identification. In infrared-welded assemblies, black pigment increases IR absorption and may reduce weld cycle time compared with natural or light-coloured variants. Batch-to-batch variation in colour concentrate loading should be monitored when the mould has melt-flow-sensitive thin-wall features because black concentrate can alter solidification rate and gate freeze-off time.
Under IEC 60695-11-10:2013, PBT-FR 1403G6 GBK4 is classified as UL 94 V-0 at 0.75 mm and 1.5 mm nominal thickness; some production lots may maintain V-0 at 0.4 mm, but end-use certification must be confirmed at the final wall thickness. Glow-wire flammability index is typically 960°C at 1.0 mm and glow-wire ignition temperature 775°C at 1.0 mm under IEC 60695-2-12 and IEC 60695-2-13. Comparative tracking index is usually 250–300 V under IEC 60112:2020, which places the compound in the PLC 3 to PLC 2 range for material-level tracking performance. Dielectric strength of 2.0 mm specimens is typically 20–24 kV/mm under IEC 60243-1. The glass fibre and flame-retardant package reduce CTI relative to unfilled PBT; designs requiring CTI above 600 V or a PLC 0 rating should use an unfilled or mineral-filled grade. The product should not be considered halogen-free; the FR designation does not imply halogen-free performance and the compound must not be used where halogen-free electrical and electronic equipment specifications apply. After thermal ageing of 1,000 h at 140°C, tensile strength retention may be 70–85% depending on air velocity and specimen thickness.
| Parameter | Unit | Range | Equipment or standard |
|---|---|---|---|
| Residual moisture after drying | % | ≤0.02 | ISO 15512:2022 method B |
| Dryer dew point | °C | ≤−30 | Desiccant dryer |
| Pre-dry temperature | °C | 120–140 | Hopper dryer |
| Melt temperature | °C | 245–270 | Nozzle pyrometer |
| Mould temperature | °C | 60–100 | Water or oil temperature control unit |
| Back pressure | MPa | 0.3–0.7 | Hydraulic system |
| Screw peripheral speed | m/min | 5–10 | Three-zone screw |
| Melt residence time | min | ≤8 | At melt temperature |
| Screw L/D ratio | ratio | 20:1–24:1 | General-purpose screw |
| Compression ratio | ratio | 2.5:1–3.0:1 | General-purpose screw |
| Property | Unit | Test method | Representative range |
|---|---|---|---|
| Density | g/cm³ | ISO 1183-1:2019 | 1.66–1.70 |
| Tensile strength at break | MPa | ISO 527-1/-2:2012 | 105–120 |
| Tensile elongation at break | % | ISO 527-1/-2:2012 | 2.0–2.5 |
| Flexural strength | MPa | ISO 178:2019 | 170–190 |
| Flexural modulus | MPa | ISO 178:2019 | 8,500–9,800 |
| Charpy notched impact at 23°C | kJ/m² | ISO 179-1/1eA:2023 | 7–9 |
| Heat deflection temperature at 1.80 MPa | °C | ISO 75-1/-2:2020 | 195–205 |
| UL 94 flammability class | class | IEC 60695-11-10:2013 | V-0 at 0.75 mm |
| Comparative tracking index | V | IEC 60112:2020 | 250–300 |
| Melt volume-flow rate at 250°C/2.16 kg | cm³/10 min | ISO 1133-1:2022 | 8–15 |
| Mould shrinkage, flow direction | % | ISO 294-4:2018 | 0.2–0.6 |
| Mould shrinkage, transverse direction | % | ISO 294-4:2018 | 0.7–1.2 |
Production-scale connector housings moulded in PBT-FR 1403G6 GBK4 are used in relay bases, power distribution blocks, terminal strips, and automotive under-hood connectors. The 30 wt% glass fibre provides dimensional stability after thermal cycling between −40°C and 150°C and reduces creep under bolt loads; however, notch sensitivity increases relative to unfilled PBT. Sharp internal corners below 0.5 mm radius should be avoided in mould design because stress concentration at glass-fibre ends initiates cracking under vibration. In connectors with press-fit pins, hole diameters must account for low elongation at break to avoid hoop-stress fracture during pin insertion. In thin-wall relay bases with wall thickness below 1.0 mm, flow length is limited by glass fibre and flame-retardant filler; short shots at flow length-to-thickness ratios above 120:1 are possible unless multiple gates are used.
Regulatory compliance should be confirmed against the lot-specific certificate. The compound generally meets RoHS Directive (EU) 2015/863 restrictions on lead, cadmium, mercury, hexavalent chromium, polybrominated biphenyls, and polybrominated diphenyl ethers, but the flame-retardant package composition must be verified because brominated systems can contain regulated impurities if not controlled. REACH SVHC declarations are lot-specific. For food-contact or medical devices, the grade is not recommended; it is not supplied with EU 10/2011 or USP Class VI documentation. The material is not suited for prolonged contact with hot water, strong bases, or amine-rich coolants above 60°C because PBT hydrolyses; glycol-based coolants and aggressive automotive fluids can stress-crack moulded parts. Painting and adhesive bonding require surface treatment because the moulded surface has low polar free energy; plasma or corona pre-treatment increases bond strength. Published data for adhesion of this exact GBK4 variant to polyurethane adhesives is limited.