| HS Code | 431317 |
| Product Name | Nan Ya PBT-FR 1403G6 |
| Polymer Type | Polybutylene Terephthalate (PBT) |
| Filler Reinforcement | 30% Glass Fiber |
| Flame Retardancy | UL94 V-0 |
| Density | 1.65 g/cm3 |
| Tensile Strength | 110 MPa |
| Elongation At Break | 2.0% |
| Flexural Modulus | 8500 MPa |
| Notched Izod Impact Strength | 7 kJ/m2 |
| Heat Deflection Temperature At 1 8 Mpa | 200 °C |
| Volume Resistivity | 1E16 ohm·cm |
| Dielectric Strength | 20 kV/mm |
| Mold Shrinkage | 0.2-0.5% |
| Processing Melt Temperature | 240-260 °C |
| Drying Temperature | 120 °C |
As an accredited Nan Ya PBT-FR 1403G6 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Nan Ya PBT-FR 1403G6 is packed in 25 kg moisture-resistant paper bags, typically 40 bags per shrink-wrapped pallet (1,000 kg). |
| Container Loading (20′ FCL) | 20′ FCL container loading of Nan Ya PBT-FR 1403G6 with proper palletization, lashing, and moisture protection for safe ocean transport. |
| Shipping | Nan Ya PBT-FR 1403G6 is supplied as flame-retardant, glass-fiber-reinforced PBT pellets in sealed 25 kg moisture-barrier bags, palletized and stretch-wrapped. It is not regulated as dangerous goods for DOT, IMDG, or IATA transport. Keep dry, cool, and out of direct sunlight; follow the SDS and local regulations. |
| Storage | Store in a cool, dry, well-ventilated area in tightly sealed original containers. Keep away from direct sunlight, heat, open flames, and strong oxidizing agents. Protect from moisture and contamination; avoid dust generation. Do not store near food, drink, or animal feed. Follow SDS/local regulations and use first-in, first-out. |
| Shelf Life | Shelf life is typically 12 months in original sealed packaging, stored cool and dry; protect from moisture and direct sunlight. |
Competitive Nan Ya PBT-FR 1403G6 prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Nan Ya PBT-FR 1403G6 is a glass-fiber-reinforced flame-retardant polybutylene terephthalate molding compound. The grade designation indicates a nominal glass-fiber loading of 30 wt% and a halogenated flame-retardant system. The pellets are used primarily for injection molding of electrical and electronic components that require UL 94 V-0 certification at 0.8 mm and 1.6 mm wall thickness. The material is not intended for direct food-contact use or for conditions exceeding the thermal stability limit of the flame-retardant package. Publicly available data for this specific configuration is limited compared with general-purpose PBT grades; the manufacturer’s certificate of analysis and current UL yellow card remain the normative references for lot-level values.
Incoming pellets typically contain residual moisture between 0.06 wt% and 0.12 wt%. Pre-drying at 120 °C for 4 h in a desiccant dryer reduces moisture below 0.02 wt%, which is the commonly accepted threshold for glass-reinforced PBT before melt processing. Dew point of the drying air should remain below -30 °C. In production areas where ambient relative humidity exceeds 60%, dry-to-mold conveying is recommended because pellet moisture regain can exceed 0.03 wt% within 30 min in an open hopper. If melt-phase moisture exceeds 0.03 wt%, hydrolysis lowers molecular weight, reduces notched impact strength, and widens lot-to-lot viscosity variation. The grade should not be blended with acetal, polyamide, or unneutralized amine-based masterbatches; interaction with the halogenated flame-retardant system can disrupt V-0 performance and produce gas voids at weld lines.
The flame-retardant package changes density, melt rheology, stiffness, ductility, and electrical tracking behavior relative to non-flame-retardant PBT. A representative property envelope for this compound class is given below. Values are conditional on specimen conditioning at 23 °C and 50% RH following ISO 291. Pigment loading and regrind content can shift these values lot-to-lot.
| Property | Test method | Typical range | Unit |
|---|---|---|---|
| Density | ISO 1183-1:2019 | 1.59–1.63 | g/cm³ |
| Tensile stress at break | ISO 527-2:2012 | 95–110 | MPa |
| Tensile modulus | ISO 527-2:2012 | 8.0–10.0 | GPa |
| Flexural strength | ISO 178:2019 | 150–170 | MPa |
| Flexural modulus | ISO 178:2019 | 7.5–9.0 | GPa |
| Charpy notched impact strength | ISO 179-1/1eA | 6–8 | kJ/m² |
| Heat deflection temperature at 1.8 MPa | ISO 75-2/Af | 200–210 | °C |
| Melt volume-flow rate at 250 °C and 2.16 kg | ISO 1133-1:2022 | 15–25 | cm³/10 min |
Mechanical behavior after injection molding is anisotropic because glass fibers orient predominantly along the flow direction. Flow-direction tensile strength is commonly 10–20% higher than cross-flow tensile strength. Molded plaques of 2 mm thickness with a single end gate can show flow-direction mold shrinkage from 0.2% to 0.4% and cross-flow shrinkage from 0.7% to 1.0%, depending on mold temperature and packing. The shrinkage differential is larger than that of unfilled PBT and should be addressed by gate placement, runner balance, and cooling-channel layout.
Flame-retardant certification is based on the UL 94 vertical burn test. The grade achieves V-0 at 0.8 mm and 1.6 mm in the certified black and natural series when molded inside the supplier’s specified process window. For components with wall thickness below 0.4 mm, the V-0 listing should not be extrapolated without a separate UL 94 evaluation. The flame-retardant mechanism involves halogen-antimony species; thermal decomposition evolves antimony trihalides and hydrogen halide gases. This decomposition pathway limits melt temperature and residence time.
Electrical tracking resistance on equivalent halogenated 30% glass-filled PBT grades is typically between 200 V and 250 V under IEC 60112. Halogen-free 30% glass PBT grades can exceed 500 V under the same test. Therefore, designs with narrow creepage distances or polluted overvoltage conditions should be assessed under IEC 60664-1 rather than relying only on UL 94 V-0. Dielectric strength on equivalent materials under IEC 60243-1 is generally 20–25 kV/mm at 2 mm thickness. Volume resistivity may exceed 10¹⁴ Ω·cm at 23 °C but can fall to approximately 10¹² Ω·cm at 80 °C and 80% RH. Component-level dielectric withstanding voltage tests remain mandatory because glass-fiber orientation and weld lines can create local weak points.
Chemical resistance follows the PBT matrix in most non-alkaline environments. The compound resists gasoline, diesel, glycol coolants, and many industrial oils at temperatures up to 60 °C. Strong alkalis, hot water above 80 °C, and amine-based cleaning agents can hydrolyze the polymer and extract antimony species from the flame-retardant package. Long-term exposure to damp heat at 85 °C and 85% RH should be validated because such conditions can reduce molecular weight and degrade electrical properties. Short-term exposure to soldering temperatures is not recommended; the crystalline melting point of PBT is approximately 223 °C, and connector housings can distort above 200 °C under load.
Melt temperature at the nozzle should be held between 240 °C and 260 °C. Barrel profiles typically rise from 200 °C in the feed zone to 250–260 °C at the nozzle. The feed throat should remain water-cooled below 60 °C to prevent pellet bridging and premature flame-retardant softening. Mold temperature should be set between 40 °C and 80 °C; the upper range improves surface gloss and dimensional stability but lengthens cycle time. Back pressure between 0.2 MPa and 0.5 MPa improves glass-fiber and flame-retardant dispersion without excessive shear heating. Screw speed should be kept below 80 rpm on typical 40 mm to 60 mm screw diameters to limit fiber attrition. Holding pressure is normally 60–80% of peak injection pressure, but the value must be determined by gate-seal time on the production tool.
Residence time must be minimized. At 260 °C, the melt should not remain in the barrel for more than 5 min during interruption. Extended residence accelerates evolution of antimony halides and hydrogen bromide, causing black specks, viscosity loss, and corrosion of carbon steel. For continuous runs exceeding 48 h, supplier technical bulletins specify nitrided or bimetallic barrels, corrosion-resistant mold steels, and closed-loop venting. Shutdown should be performed using a purging compound that is thermally stable and free of halogenated flame retardants. If the compound is left in a hot barrel during unplanned downtime, acidic condensate can form on screw and check-ring surfaces.
Thin-wall parts with flow length-to-thickness ratios above 150 generally require mold temperatures at the upper end of 80 °C and injection speeds up to 300 mm/s. High shear rates above 10,000 s⁻¹ can break glass fibers and reduce mechanical strength. Mold trials with cavity pressure sensors in the range 30–50 MPa are used to confirm packing and gate freeze. Premature release of hold pressure can produce sink marks near bosses and ribs. For a projected area of 100 cm², clamp force demand can rise by 5–10% relative to a non-flame-retardant 30% glass PBT because of the higher melt viscosity of the flame-retardant system.
Batch-release testing for this grade class includes density, melt flow rate, tensile strength, notched impact, heat deflection temperature, and UL 94 vertical burn. Injection molders should also verify pellet moisture, color variation, and flow length. Regrind ratios are commonly limited to 25%; higher regrind levels can reduce V-0 repeatability and produce surface streaks. Glass-fiber length after molding is typically reduced to 250–350 µm from longer pellet-level fiber length because of screw shear. This reduction is normal but must be monitored because excessive fiber attrition lowers modulus and heat deflection temperature.
The substitution requires revalidation of filling, packing, dimensional stability, and flammability. The flame-retardant compound has different density and melt rheology. The same screw-position setpoint may not produce the same cushion, so switch-over point should be reset using short-shot studies. Small edge gates below 0.8 mm in thickness can freeze prematurely and intensify jetting or surface roughness. Runner diameter and sprue bushing orifice may need enlargement because the compound fills less readily than a non-flame-retardant 30% glass PBT of equivalent filler loading.
Compared with unfilled flame-retardant PBT, the 30% glass grade increases tensile strength from roughly 50–60 MPa to 95–110 MPa and flexural modulus from roughly 2.5–3.0 GPa to 7.5–9.0 GPa. This improves retention of connector latches, terminal pins, and threaded inserts under vibration. Elongation at break, however, falls below 3%, reducing applicability for snap-fit features that require high strain. Compared with a 15% glass-reinforced flame-retardant PBT, the 30% glass grade has higher heat deflection temperature and lower mold shrinkage but lower notched impact strength and greater shrinkage anisotropy.
Compared with non-flame-retardant 30% glass PBT, the halogenated flame-retardant system raises density by approximately 0.06–0.10 g/cm³ and reduces tensile strength by approximately 10–20%. Flow length also decreases because brominated flame-retardant and antimony trioxide increase filler volume fraction. For water-absorbing engineering resins such as 30% glass-reinforced polyamide 66, mechanical properties shift significantly between dry-as-molded and conditioned states. Under ISO 62, PBT absorbs approximately 0.1% water after 24 h, so dimensions and dielectric properties remain more stable in humid service. Halogen-free flame-retardant PBT grades may reduce regulatory burden but often require different melt temperatures and can exhibit different tracking resistance. Published data for this specific configuration is limited in public databases; direct material-to-material replacement must be validated on the production tool under the final molded wall thickness.
Regulatory compliance must be confirmed against the supplier’s current declaration. Under RoHS 2011/65/EU Annex II, the relevant restricted substances are maintained below thresholds when tested by IEC 62321-5 or XRF screening. Under REACH EC 1907/2006, the presence of candidate-list flame-retardant additives must be verified by the supplier for each lot because formulations can change. The material is not covered by a food-contact grade approved under FDA 21 CFR 177.1660 because the flame-retardant system is not typically included in that specification. Applications requiring UL 94 V-0 at wall thickness below 0.4 mm, or CTI values above 250 V, should not be assigned to this grade without additional testing.
Application candidates include connector housings, relay bases, terminal blocks, motor end caps, and enclosures for low-voltage switchgear. For each component, ignition resistance should be evaluated to IEC 60695-11-10 or UL 94, tracking behavior to IEC 60112, and dimensional stability to the applicable product standard. The combination of 30 wt% glass reinforcement and V-0 at 0.8 mm supports compact electrical insulation when molded under the specified drying and melt-temperature limits. Parts with thin ribs below 0.5 mm and long flow paths may require mold-flow simulation using measured shear-viscosity data rather than generic PBT material data.