| HS Code | 627907 |
| Density | 1.53 g/cm³ |
| Filler Content | 30% glass fiber |
| Water Absorption | 0.07% |
| Molding Shrinkage | 0.2-0.5% |
| Tensile Strength | 100 MPa |
| Elongation At Break | 2.0% |
| Flexural Modulus | 8500 MPa |
| Flexural Strength | 150 MPa |
| Notched Impact Strength | 8 kJ/m² |
| Heat Deflection Temperature At 1 8 Mpa | 200 °C |
| Ul94 Flammability | V-0 |
| Dielectric Strength | 20 kV/mm |
| Volume Resistivity | 1E15 Ω·cm |
| Melting Point | 225 °C |
As an accredited Nan Ya PBT-FR 1403G3 GBK4 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Nan Ya PBT-FR 1403G3 GBK4 is packaged in 25 kg moisture-proof bags, typically 40 bags per pallet. |
| Container Loading (20′ FCL) | Nan Ya PBT-FR 1403G3 GBK4 is loaded in a clean, dry 20′ FCL, palletized in sealed bags and secured for safe ocean transport. |
| Shipping | Nan Ya PBT-FR 1403G3 GBK4 is a black, flame-retardant, glass-fiber-reinforced polybutylene terephthalate compound supplied as plastic pellets. It is shipped as a non-hazardous solid resin in sealed bags, boxes, or bulk containers, protected from moisture, heat, and direct sunlight under normal industrial handling conditions. |
| Storage | Store Nan Ya PBT-FR 1403G3 GBK4 in a cool, dry, well-ventilated area away from direct sunlight, heat, sparks, and open flames. Keep containers tightly closed to prevent moisture pickup and contamination. Protect bags from punctures, dust, and physical damage. Maintain stable temperature and humidity, use first-in, first-out stock rotation, and follow the SDS and local storage regulations. |
| Shelf Life | Store in a cool, dry place; under normal conditions it is stable, with a typical shelf life of two years. |
Competitive Nan Ya PBT-FR 1403G3 GBK4 prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Nan Ya PBT-FR 1403G3 GBK4 is a flame-retardant polybutylene terephthalate injection-moulding compound reinforced with 30 wt% glass fibre and supplied with a black colourant package. In the Nan Ya PBT nomenclature, the G3 digit conventionally denotes a 30 wt% glass-fibre loading, while GBK4 identifies the colour and additive package; the exact flame-retardant chemistry is not disclosed by the grade designation and must be confirmed from the safety data sheet and lot certificate. Published product-specific data for this exact black designation are limited in open repositories, so the processing and property statements below use the general class of flame-retardant PBT-GF30 and the supplier’s certificate of analysis for design verification.
This product class is specified where dimensional stability, flexural stiffness, and flammability certification must be satisfied in a single feedstock. Typical class-level density for 30 wt% glass-reinforced flame-retardant PBT lies in the range 1.55–1.65 g/cm³ under ISO 1183-1; glass-fibre content is confirmed by ash testing under ISO 3451-1. Incoming resin is often compared on melt-volume-flow rate under ISO 1133-1 at 260 °C and 2.16 kg, but parity between supplier and moulder must be established because moisture content and shear history shift the observed value.
Because the grade is frequently specified for current-carrying insulation in connectors, terminal blocks, relay sockets, coil bobbins, and miniature circuit-breaker internal parts, the first qualification hurdle is usually the vertical burning test under UL 94. Flame-retardant PBT-GF30 materials of this class are conventionally certified to UL 94 V-0 at a wall thickness of 0.75 mm; a thicker section such as 1.5 mm may also be certified but does not automatically guarantee thin-wall performance, because the flame-retardant additive package and glass-fibre wicking at the surface control burn time and dripping behaviour. Comparative tracking index under IEC 60112 generally falls between 250 V and 450 V for this product family, depending on the FR package; lot-specific values must be taken from the certificate of analysis. Glow-wire ignition temperature under IEC 60695-2-10 is a further qualification requirement for unattended appliance housings and relay bases.
In production, the limiting parameter is hydrolytic stability rather than melt strength. The compound must be dried to a residual moisture content below 0.02 wt% in a dehumidifying hopper dryer with a supply-air dew point of −30 °C or lower; a common drying setpoint is 120–130 °C for 3–4 h, but only a moisture analyser can confirm readiness. PBT ester linkages are subject to hydrolysis at processing temperatures, and retained moisture produces gas jets, silver streaking, and a reduction in tensile strength that may not be visible until subsequent environmental testing.
Barrel temperatures from the feed zone to the nozzle are generally profiled between 245 °C and 265 °C, with the nozzle held near 255 °C; melt temperatures above 270 °C should be avoided because flame-retardant decomposition can generate plate-out, screw torque fluctuation, and free surface contamination on tool surfaces. Total residence time in the barrel should not exceed 5 min; if machine interruption exceeds this boundary, the heat-soaked melt should be purged rather than retained for further moulding. Screw geometry suitable for glass-reinforced flame-retardant PBT is a general-purpose or low-compression design with an L/D ratio of 20:1 to 24:1 and a compression ratio of 2.5:1 to 3.5:1. Glass-fibre length is shear-sensitive; high-shear screw tips, undersized sprue bushings, and excessive back pressure will comminute fibres and reduce load-bearing capability. Back pressure is normally limited to 0.3–0.7 MPa, and injection pressure at transfer is commonly 80–120 MPa for multi-cavity connector work, although part geometry and flow path determine the actual hydraulic demand.
Mould temperature is maintained between 60 °C and 90 °C to control crystallinity, surface finish, and post-mould dimensional drift. Lower tool temperatures produce faster solidification but may reduce weld-line strength and increase internal stress. A hold pressure of 50–70% of the peak injection pressure, with hold time sufficient to seal the gate and compensate solidification shrinkage, is typical for parts with wall sections below 2.5 mm. Venting depth on the parting line should be limited to approximately 0.02–0.03 mm to prevent gas burns from flame-retardant decomposition volatiles without creating flash.
From a comparative standpoint, the 30 wt% glass phase primarily alters mould shrinkage, flexural modulus, and heat deflection temperature. The glass-reinforced flame-retardant PBT has roughly 2.5–3.5 times the flexural modulus of an unfilled flame-retardant PBT and a heat deflection temperature under 1.8 MPa that is approximately 2.5 times higher. The trade-off appears in failure mode: the glass-filled system is stronger in load-bearing applications but is more anisotropic, more notch-sensitive in thin sections, and more dependent on fibre orientation than the unfilled analogue.
| Characteristic | Flame-retardant PBT-GF30 class | Unfilled flame-retardant PBT | Non-flame-retardant PBT-GF30 |
|---|---|---|---|
| Density (ISO 1183-1) | 1.55–1.65 g/cm³ | 1.35–1.45 g/cm³ | 1.50–1.60 g/cm³ |
| Tensile strength (ISO 527-2) | 100–130 MPa | 50–70 MPa | 105–135 MPa |
| Flexural modulus (ISO 178) | 8000–10000 MPa | 2500–3000 MPa | 7500–9500 MPa |
| Heat deflection temperature at 1.8 MPa (ISO 75-2) | 195–215 °C | 60–80 °C | 190–210 °C |
| Notched Charpy impact (ISO 179-1/1eA) | 7–10 kJ/m² | 3–5 kJ/m² | 8–12 kJ/m² |
| UL 94 rating at 0.75 mm | V-0 | V-0 | HB |
Against a non-flame-retardant PBT-GF30, the flame-retardant package increases density and generally reduces notched impact and melt elongation; the benefit is the established UL 94 rating at thin wall sections, which a non-FR PBT-GF30 typically cannot meet. Against an unfilled flame-retardant PBT, the glass fibre increases modulus and heat deflection temperature but lowers spiral-flow length and introduces anisotropic shrinkage.
For tool design, post-mould shrinkage must be measured under ISO 294-4 and not taken as an isotropic value. In glass-reinforced PBT, shrinkage parallel to the glass-fibre orientation is class-typically 0.2–0.4%, while shrinkage transverse to flow may be 0.7–1.0%; the differential creates warpage in flat, gated parts and must be compensated by gate placement and cooling-circuit layout. Unfilled flame-retardant PBT shrinks more uniformly but at a higher absolute level, so a tool cut to unfilled-PBT shrinkage is generally unsuitable for direct conversion without dimensional allowance changes.
Under those conditions, moisture absorption becomes the dominant selection criterion. Polybutylene terephthalate absorbs substantially less water than polyamide 66; class-level equilibria under ISO 62 at 23 °C and 50% relative humidity are commonly 0.2–0.4% for PBT-GF30 formulations, whereas PA66-GF25 may equilibrate in the region of 1.5–2.0%. The consequence appears not only as dimensional growth but also as time-dependent depression of glass-transition and load-bearing performance in the polyamide. In PBT, the lower moisture uptake reduces humidity-driven changes in dimensions and electrical tracking behaviour in connectors that operate in partially sealed enclosures. The trade-off is that PA66-GF25 may offer higher dry-state heat deflection temperature and greater ductility; therefore substitution into a part originally qualified for PA66-GF25 requires a re-evaluation of snap-fit strain limits under ISO 527-2 rather than a simple drop-in material substitution.
At gate locations and flow-field transitions in multi-cavity tools, the orientation of the 30 wt% glass fibre phase imposes anisotropic tensile behaviour that is difficult to capture from datasheet measurements alone. The weld line formed when two melt fronts meet after a pin, slot, or multi-gate filling pattern can reduce the tensile strength of glass-filled PBT by 30–50% relative to the nominal material value, because the fibres align parallel to the weld plane rather than bridging it. In connector housings with holes in the mating face, the gate location should be positioned so that the weld line is forced into a low-stress region or eliminated by a sequential valve-gate system. Increasing the mould temperature toward the upper limit of 90 °C and using higher injection speed can improve weld-line strength by delaying flow-front solidification, but fibre attrition may rise if the injection speed is increased without adjusting the nozzle and sprue diameter. Published data for the exact GBK4 designation under defined gating configurations is limited; part-specific weld-line testing under ISO 527-2 is necessary for design verification.
Because OEM standards for electrical enclosures increasingly distinguish between RoHS compliance and halogen-free construction, the flame-retardant chemistry of Nan Ya PBT-FR 1403G3 GBK4 must be verified before release. The IEC 61249-2-21 halogen-free definition limits chlorine to 900 ppm, bromine to 900 ppm, and total chlorine plus bromine to 1500 ppm. A brominated flame-retardant package with antimony trioxide synergist can be fully compliant with RoHS Directive 2011/65/EU Annex II while failing that halogen-free threshold; therefore compliance data must cover both frameworks separately. If the application requires halogen-free declaration, a direct substitution to a non-halogen flame-retardant PBT-GF30 does not guarantee the same melt rheology, comparative tracking index, or impact behaviour, because non-halogen systems may require higher additive loadings. The substitution should be re-qualified for UL 94 at the minimum part wall thickness and for IEC 60112 CTI, with special attention to mould deposit formation and screw torque during extended runs.
For continuous-use thermal evaluations, electrical insulation systems often rely on the relative thermal index under UL 746B. Glass-reinforced flame-retardant PBT can carry an RTI in the range of 120–140 °C for electrical properties, depending on the specific formulation and colourant package; the value is not a processing temperature and does not imply retention of full mechanical properties. The exact RTI for Nan Ya PBT-FR 1403G3 GBK4 should be read from the UL Yellow Card, not inferred from class-level data.
Closed-loop regrind in hot-runner connector moulds introduces a second thermal and shear history that reduces the glass-fibre length and broadens the fibre-length distribution. In production-scale trials, regrind fractions above 20 wt% may reduce tensile strength by 5–10% and notched impact by a larger percentage, although the exact loss depends on gate geometry, regrind particle size, and whether the material passes through a hot-runner manifold. The melt-volume-flow rate under ISO 1133-1 at 260 °C and 2.16 kg typically increases with regrind content because fibre attrition lowers melt viscosity; an increase above the supplier’s virgin specification may indicate excessive chain scission or flame-retardant degradation. Operators should therefore blend regrind at or below the limit stated on the lot certificate, monitor ash content under ISO 3451-1 to confirm glass loading, and reject lots that show black specks, yellowing, or a change in UL 94 burning behaviour. If a high-temperature soak occurs, the material should be purged rather than mixed into the feed stream.