| HS Code | 562483 |
| Density | 1.35 g/cm³ |
| Melt Flow Rate | 20 g/10 min (250°C/2.16 kg) |
| Tensile Strength | 50 MPa |
| Tensile Elongation At Break | 30% |
| Flexural Modulus | 2300 MPa |
| Flexural Strength | 80 MPa |
| Charpy Notched Impact Strength | 3 kJ/m² |
| Heat Deflection Temperature At 0 45 Mpa | 150 °C |
| Heat Deflection Temperature At 1 82 Mpa | 70 °C |
| Vicat Softening Temperature | 200 °C |
| Flammability Rating | UL94 V-0 (0.75 mm) |
| Water Absorption | 0.08% |
| Mold Shrinkage | 0.4–0.8% |
| Volume Resistivity | 1E16 Ω·cm |
| Dielectric Strength | 20 kV/mm |
| Dielectric Constant | 3.0 |
| Dissipation Factor | 0.002 |
| Rockwell Hardness | R115 |
As an accredited Mitsubishi Engineering Plastics Lumiloy® PBT Unfilled GN2250 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Mitsubishi Engineering Plastics Lumiloy® PBT Unfilled GN2250 is supplied in 25 kg moisture-barrier bags, 40 bags per pallet. |
| Container Loading (20′ FCL) | 20′ FCL container loading for Mitsubishi Engineering Plastics Lumiloy® PBT Unfilled GN2250: palletized bags, shrink-wrapped, secured, and evenly distributed for ocean transport. |
| Shipping | Mitsubishi Engineering Plastics Lumiloy® PBT Unfilled GN2250 is generally shipped as non-hazardous polymer resin in sealed moisture-barrier bags or boxes, palletized and kept dry. Avoid heat, sunlight, and moisture during transport; handle with care and follow local freight regulations. |
| Storage | Store Lumiloy® PBT Unfilled GN2250 in a dry, cool, well-ventilated area away from direct sunlight, heat, and ignition sources. Keep in original sealed packaging to prevent moisture absorption and contamination. Avoid contact with strong oxidizers. Maintain stable ambient conditions and follow first-in, first-out inventory practices. Use dry-handling procedures; if moisture uptake is suspected, dry resin per supplier recommendations before processing. |
| Shelf Life | For Lumiloy® PBT GN2250, shelf life is typically 12 months when stored dry in unopened original packaging, away from heat and moisture. |
Competitive Mitsubishi Engineering Plastics Lumiloy® PBT Unfilled GN2250 prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Lumiloy® PBT Unfilled GN2250 is a non-flame-retardant, unreinforced polybutylene terephthalate injection-molding grade supplied by Mitsubishi Engineering-Plastics Corporation. The product is intended for electrical insulation and electromechanical components such as relay bobbins, transformer coil formers, terminal blocks, connector housings, switch components, and motor-insulating frames. The semicrystalline polyester structure provides rapid crystallization, low water absorption, and stable dielectric response in dry-service conditions. The melting range is approximately 225°C, and the normal melt-processing range is 240–260°C. Published property values for the exact GN2250 lot must be confirmed against the production certificate and UL Yellow Card; the following sections consolidate representative class data for unfilled PBT rather than a supplier-guaranteed specification.
The unfilled grade differs from glass-fiber-reinforced Lumiloy variants primarily in stiffness, heat deflection temperature, and mold-shrinkage anisotropy. Glass-filled PBT at 30% fiber loading typically shifts flexural modulus from the unfilled range of 2.3–2.8 GPa to 8–10 GPa and raises heat deflection temperature at 1.80 MPa from about 55–65°C to 200–215°C. That increase in load-bearing capacity is accompanied by reduced elongation, higher tool wear, and greater warpage driven by fiber orientation. GN2250 is therefore evaluated where low warpage, thin-wall filling, electrical tracking resistance, and dimensional stability under humid exposure are more critical than structural stiffness.
Unfilled PBT ester linkages undergo hydrolysis through a pseudo-first-order reaction that accelerates sharply with temperature and absorbed moisture. At melt temperatures above 250°C, residual moisture above 0.02% by mass is sufficient to reduce molecular weight, produce silver streaks and voids, and lower notched impact and dielectric breakdown performance. Production-scale drying must use a closed-loop desiccant hopper dryer with a return-air dew point no higher than -30°C. Granulate should be dried at 120°C for 4–6 h or 130°C for 3–4 h to reach the target moisture content. Hopper seals, drying capacity, and dew-point stability are critical; leakage or dew-point drift above -20°C is a recurring cause of intermittent short-shot rejection in thin-wall connector tools.
After drying, granulate should be conveyed with dry air and maintained under a dry-air purge at the machine feed throat. Barrel residence time above 260°C should not exceed 8–10 min during normal cycling. For hot-runner tools, manifold and nozzle temperatures are set to 250–260°C with zone-to-zone variation of no more than ±2°C. Because unfilled PBT viscosity is temperature-sensitive, unbalanced hot-runner zones can increase weld-line depth and cavity-to-cavity fill variation that later appears as dimensional scatter under ISO 294-4.
On injection machines with screw diameters from 18–25 mm and 20:1 L/D general-purpose polyolefin screws, a typical barrel profile is 230°C rear, 245°C center, 255°C front, and 255°C nozzle. Melt temperature should not exceed 270°C during normal cycling, and hot-runner residence time should remain below 10 min. Back pressure of 0.5–1.0 MPa and screw surface speed of 50–150 mm/s are adequate for melt homogeneity without excessive shear heating. Mold temperature is normally set from 40–80°C, with 60°C commonly used to balance cycle time and degree of crystallinity.
Published data for the specific GN2250 configuration is limited; the following property envelope is based on the unfilled PBT class and should be verified against the supplier batch certificate.
| Property | Test Method | Representative Unfilled PBT Envelope |
|---|---|---|
| Density | ISO 1183-1 | 1.30–1.32 g/cm³ |
| Tensile stress at yield | ISO 527-2:2012 | 50–60 MPa |
| Tensile strain at break | ISO 527-2:2012 | >50% |
| Flexural modulus | ISO 178:2019 | 2.3–2.8 GPa |
| Flexural strength | ISO 178:2019 | 80–90 MPa |
| Charpy notched impact at 23°C | ISO 179-1/1eA:2023 | 3–5 kJ/m² |
| Heat deflection temperature at 0.45 MPa | ISO 75-2/B:2020 | 140–160°C |
| Heat deflection temperature at 1.80 MPa | ISO 75-2/A:2020 | 55–65°C |
| Comparative tracking index | IEC 60112:2020 | 600 V |
| Volume resistivity | IEC 62631-3-1:2016 | >1 × 1014 Ω·m |
| Dielectric strength | IEC 60243-1:2013 | 15–20 kV/mm |
| Mold shrinkage | ISO 294-4:2018 | 1.4–2.0% |
| Water absorption at 24 h/23°C | ISO 62:2008 | 0.08% |
| Flammability | UL 94 | HB at thickness per Yellow Card |
Values are not specification limits. Pigmentation, additive stabilization, moisture state, and specimen preparation can shift notched impact by approximately ±1 kJ/m² and heat deflection temperature by ±5°C. The manufacturer’s lot certificate and UL Yellow Card remain the controlling documents for supplied material.
In production tools with cavity counts from 4 to 32 and wall thickness below 1.0 mm, the practical flow length to wall thickness ratio for unfilled PBT is generally in the range of 150:1 to 200:1 at normal melt temperatures. Beyond this range, short shots, flow hesitation, and brittle weld lines become probable. Gate freeze time is short in this polyester; hold-pressure time should be established from cavity pressure decay or gate-sealing studies rather than fixed timers. Direct edge gates or submarine gates with land lengths of 0.5–1.0 mm and diameters of 0.8–1.2 mm are common for wall sections from 0.8–2.5 mm. For high-cavitation connectors, valve-gated hot-runner systems are preferred because unheated runners freeze before pack pressure can complete crystallization.
Mold temperature is a critical control variable. A tool temperature of 60°C is commonly specified to balance cycle time and crystallinity development. Mold temperatures below 40°C can freeze the part surface before full crystallization, increasing post-mold dimensional movement and reducing heat-aging stability under service temperature. When metallic inserts are overmolded, insert preheat to 100–130°C is used to reduce residual stress; insert temperatures below 80°C can produce sink marks, stress concentration, and localized electrical weakness at the metal-polymer interface. Cavity pressure sensors should monitor post-fill pressure decay and verify that the gate freezes before holding pressure is released.
The unreinforced grade has a flexural modulus in the range of 2.3–2.8 GPa, while glass-fiber-reinforced PBT grades at 30% loading generally exceed 8 GPa. The reinforced grades also provide substantially higher load-bearing capacity and lower mold shrinkage, but their fiber orientation creates anisotropic shrinkage and warpage in complex geometries. GN2250 is therefore selected for precision electrical parts where dimensional consistency and low residual stress are more important than maximum stiffness.
Relative to PA66, unfilled PBT absorbs much less water. The 24-h water absorption of unfilled PBT under ISO 62 is approximately 0.08%, whereas PA66 can absorb more than 1.5–2.0% at equilibrium humidity. That difference gives PBT more stable dielectric properties and dimensions in humid environments, although PA66 may offer higher dry-as-molded tensile strength and elongation. PBT also crystallizes rapidly and can permit shorter cycle times; however, the heat deflection temperature at 1.80 MPa is lower than that of many glass-filled PA66 grades.
Compared with flame-retardant PBT grades, GN2250 is non-flame-retardant and therefore does not contain the halogenated or phosphorus-based FR packages that can reduce comparative tracking index and melt flow. The trade-off is that GN2250 requires verification against end-use standards such as IEC 60695-2-12 and IEC 60695-2-13 when glow-wire or hot-wire ignition performance is required. In such cases, flame-retardant Lumiloy variants should be evaluated, but their CTI and thin-wall flow characteristics may differ from the unfilled non-FR grade.
Electrical and electronic end-use qualification typically requires a compliance matrix that links the material to specific test method designations and regulatory certificates. The matrix below summarizes the main documentation paths for GN2250-class unfilled PBT.
| Requirement | Standard or Regulatory Reference | Assessment Basis |
|---|---|---|
| Comparative tracking index | IEC 60112:2020 | 600 V typical for unfilled PBT |
| Dielectric strength | IEC 60243-1:2013 | 15–20 kV/mm |
| Flammability class | UL 94 | HB at thickness per Yellow Card |
| Melt volume-flow rate | ISO 1133-1:2022 | Reported at 250°C/2.16 kg; consult lot certificate |
| RoHS restricted substances | 2011/65/EU Annex II | Confirm against supplier certificate |
| REACH SVHC declaration | EC 1907/2006 | Confirm against supplier certificate |
The compliance documentation should be obtained from Mitsubishi Engineering-Plastics or the compounding distributor for each production lot. In particular, the UL Yellow Card thickness and color restrictions must be checked before substituting GN2250 into an existing holder design, because UL 94 ratings are thickness- and color-dependent.
On production lines manufacturing relay bobbins and connector housings, the most common processing failures observed with unfilled PBT are gate blush, flow-line discoloration from overheated hot-runner tips, and intermittent dielectric failure caused by improper drying. Gate blush is managed by reducing injection speed during the first 5–10 mm of fill and by using higher mold temperatures near the gate. Flow-line discoloration is controlled by limiting hot-runner tip temperature to 260°C and avoiding hold times above 5 min during material or color changeover. Intermittent dielectric failure, when unrelated to tool contamination, is most often traced to a hopper dryer system that is undersized for machine throughput or to granulate that has not remained at drying temperature for at least 2 h.
For connectors with wall thickness below 0.8 mm, cavity-fill imbalance can be reduced by using balanced hot-runner layouts and by maintaining nozzle temperature within ±2°C of setpoint. Published data for the exact GN2250 flow-length limit in such thin sections is limited; mold-filling simulation driven by supplier rheology data should therefore be used to establish the safe processing window before tooling is released.