| HS Code | 542532 |
| Manufacturer | Mitsubishi Engineering Plastics |
| Product Name | Lumiloy® PBT+PPS+GF AP-2110P |
| Polymer Type | PBT/PPS alloy |
| Reinforcement | Glass fiber |
| Glass Fiber Content | Approx. 10% (typical grade designation) |
| Density | Approx. 1.39 g/cm³ |
| Water Absorption | Approx. 0.02% (23°C/24 h) |
| Mold Shrinkage | Approx. 0.5–0.9% |
| Tensile Strength | Approx. 100 MPa |
| Tensile Elongation | Approx. 2.5% |
| Flexural Modulus | Approx. 5000 MPa |
| Flexural Strength | Approx. 150 MPa |
| Charpy Notched Impact Strength | Approx. 4 kJ/m² |
| Hdt At 1 82 Mpa | Approx. 195–200°C |
| Melting Point | Approx. 225°C |
| Volume Resistivity | Approx. 1×10^16 Ω·cm |
| Dielectric Strength | Approx. 20 kV/mm |
| Ul94 Flammability | HB |
| Processing Melt Temperature | Approx. 260–290°C |
| Mold Temperature | Approx. 80–120°C |
| Drying Condition | Approx. 120°C for 3–4 h |
As an accredited Mitsubishi Engineering Plastics Lumiloy® PBT+PPS+GF AP-2110P factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Packaged in 25 kg moisture-proof bags, typically palletized for industrial shipment and bulk supply. |
| Container Loading (20′ FCL) | 20′ FCL container loaded with Mitsubishi Engineering Plastics Lumiloy® PBT+PPS+GF AP-2110P, securely palletized and packed for ocean shipment. |
| Shipping | Lumiloy® AP-2110P is shipped as dry plastic pellets in sealed moisture-barrier bags, packed in cartons or octabins on pallets. Transport and store in a cool, dry area away from direct sunlight and moisture. It is not classified as dangerous goods; follow the SDS and local transport regulations. |
| Storage | Store Lumiloy® AP-2110P resin in a cool, dry, well-ventilated area away from direct sunlight, heat, and ignition sources. Keep in original sealed packaging to prevent moisture pickup and contamination. Avoid dust generation and static discharge. Do not store near incompatible chemicals. Use first-in/first-out and follow the manufacturer’s SDS for temperature, humidity, and shelf-life limits. |
| Shelf Life | Store dry, sealed, away from heat and moisture; shelf life is typically indefinite, but use within about 12–24 months under recommended conditions. |
Competitive Mitsubishi Engineering Plastics Lumiloy® PBT+PPS+GF AP-2110P prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Mitsubishi Engineering Plastics Lumiloy® AP-2110P is a glass-fiber-reinforced polybutylene terephthalate/polyphenylene sulfide blend. The designation AP-2110P identifies a material intended for injection-molded parts requiring a balance of dimensional stability, thermal resistance, and chemical resistance that exceeds conventional PBT-GF30 compounds while retaining a wider processing window than fully PPS-GF grades. Because AP-2110P contains both ester and aromatic sulfide phases, its property set is controlled by phase morphology, fiber length retention, and moisture management. The model AP-2110P should be evaluated against the manufacturer’s current datasheet and control document for batch-specific values; the following technical discussion addresses the PBT/PPS/GF compound class and the processing conditions most frequently documented for it.
Component composition in this family is not a single-phase system. The PBT phase provides melt flow, adhesion to glass-fiber sizing, and toughness; the PPS phase raises heat deflection temperature under load, reduces moisture uptake, and improves resistance to acid and hot-water exposure. Glass-fiber reinforcement increases tensile strength, flexural modulus, and creep resistance but also increases flow-direction/transverse shrinkage anisotropy. In production, these interactions are observed as lot-to-lot shifts in mold shrinkage when fiber length distribution changes at the compounding stage. Injection molders commonly use this material for connectors, sensor brackets, covers for electronic control units, cooling-circuit flanges, and pump wear surfaces where PBT-GF30 would be too moisture-sensitive and PPS-GF30 would require higher mold temperatures.
Moisture absorption in glass-reinforced PBT/PPS alloys is governed by the concentration of hydrolytically active ester linkages. Commercial PBT-GF30 grades usually show equilibrium water uptake in the range 0.1% to 0.3% after immersion at 23 °C under ISO 62. In PBT/PPS/GF compounds with equivalent fiber loading, reported moisture uptake is generally below 0.1% because PPS domains contain no ester carbonyl group and are hydrophobic. The effect is not merely surface-level: the dispersed or co-continuous PPS phase lowers the total mass fraction of degradable ester linkages and reduces moisture-induced swelling in humid environments. As a consequence, parts molded from AP-2110P are less likely to exhibit dimensional change in tropical storage or condensation cycling found in automotive interiors and engine-bay wiring interfaces.
However, the PBT phase is not fully protected. If the PPS domains are poorly dispersed, moisture can still reach the PBT phase through exposed sections, weld lines, and glass-fiber wicking at the surface. Compounding conditions must therefore be controlled to reduce PBT-rich zones at weld lines. This is one reason injection-molding trials for AP-2110P include weldline tensile specimens prepared with double-gate tooling and tested under ISO 527-2 before production release.
The usable melt temperature window for AP-2110P is bounded by the melting point of PPS on the low side and the thermal degradation rate of PBT on the high side. PPS crystals require melt temperatures of at least 280 °C to disappear and allow uniform flow; below this point, the PPS phase may remain as high-viscosity particulates that cause surface roughness, poor interphase bonding, and reduced tensile strength. At nozzle temperatures above 320 °C, the PBT ester sequences undergo chain scission at a rate that discolors the resin and reduces melt viscosity before the PPS phase reaches thermal damage. For this compound class, production settings are therefore commonly held between 285 °C and 310 °C, measured at the nozzle by a needle pyrometer with a 1 mm immersion tip. Residence time above 300 °C should not exceed 6–8 min in conventional reciprocating-screw injection machines. In hot-runner applications, unswept manifold dead spots may exceed this limit even when the press is cycling normally; hot-runner set-points below 300 °C and externally heated nozzle tips with no dead-volume pockets are required to avoid carbonized deposits and viscosity drift.
Melt pressure during filling is a secondary control because PPS-rich domains shear-thin more strongly than PBT. The effective viscosity at 1000 s⁻¹ and 290 °C is sufficiently low for filling thin walls of 0.4 mm when gate pressure is above 60 MPa; however, shear heating from excessive injection velocity above 300 mm/s can produce localized temperatures that exceed the set-point by 20–30 °C. This is a known cause of gate blush and silver streaks in PBT/PPS/GF parts. Cavity filling studies with pressure sensors in the runner and cavity are recommended during tool qualification.
Pre-drying is mandatory. The material should be dried at 120 °C to 140 °C for 4–6 h in a desiccant drier with a dew point below −30 °C; residual moisture measured by Karl Fischer titration must remain below 0.02 wt%. If the material is exposed to plant air at relative humidity above 60%, opened bags should be returned to the drier or consumed within 1 h. Moisture in the PBT phase at melt temperatures above 250 °C causes hydrolysis of the ester linkages, reducing molecular weight and tensile strength at break even when no visible splay is present. Use of general-purpose screws with 18:1 to 24:1 L/D ratio and compression ratio between 2.0:1 and 2.5:1 is acceptable for reciprocating injection machines if the screw is not operated at excessive recovery speed. Screw rotation should be limited to 60–100 mm/s surface speed to prevent glass-fiber attrition at the check ring and screw tip. Back pressure is normally set between 0.3 MPa and 0.7 MPa to homogenize the melt; higher back pressure raises melt temperature and can degrade the PBT phase during prolonged cycle interruptions.
Mold temperature should be maintained between 100 °C and 130 °C for critical dimensions. Mold temperatures below 100 °C cause PPS-rich domains to freeze before packing pressure has fully compensated volumetric shrinkage; the resulting parts show sink marks, poor knit-line fusion, and low burst strength in pressurized housings. In multi-cavity tools with hot sprues, cavity-to-cavity temperature variation above ±5 °C has been associated with differential shrinkage of 0.1–0.2% between cavities, requiring selective thermal control of core pins. Vent depths of 0.015–0.030 mm at the flow front are used to release volatiles; insufficient venting produces burn marks and carbonaceous residues at the weld line. Compounding of glass-fiber-reinforced PBT/PPS blends is generally carried out on co-rotating twin-screw extruders with L/D ratios of 40 to 48, using downstream fiber feeding to preserve fiber length and atmospheric vacuum venting at 270–300 °C.
Regrind from sprues and rejected parts may be incorporated at levels up to 20 wt% without major loss of tensile strength if the regrind is dry and particle size is consistent. Higher regrind fractions reduce fiber length distribution and alter mold shrinkage; dimensional capability data should be regenerated after any change in regrind percentage. Fiber length shortening during reprocessing is most apparent as a reduction in notched Charpy impact measured under ISO 179-1/1eA, not always as a tensile strength change.
PBT/PPS/GF components exposed to hot ethylene glycol/water mixtures at 105 °C to 130 °C encounter a hydrolytic environment that attacks the PBT phase. PBT homopolymer and PBT-GF30 grades are known to lose tensile strength after prolonged exposure to hot coolant; the PPS phase in AP-2110P restricts the propagation of ester hydrolysis by reducing the accessible ester concentration and by forming a less water-permeable domain structure. However, the material is not equivalent to a fully PPS-GF grade. If the coolant pH rises above 9.0 at 120 °C, or if high-concentration amine-based corrosion inhibitors are present, the PBT phase can undergo aminolysis and rapid molecular weight loss. Published data for this specific configuration is limited; qualification programs should include pressure-burst testing of molded housings at 140 °C and tensile testing of coolant-aged specimens under ISO 527-2.
This is an important operational boundary for AP-2110P in under-hood applications. In a typical automotive cooling-system bracket or thermostat housing, the material is selected when long-term hot-water exposure is expected to exceed PBT-GF30 limits but the part geometry and mold temperature cannot accommodate a fully PPS-GF grade. A 2.5 mm wall cooling flange with an internal metal sleeve may require a mold temperature no higher than 120 °C; AP-2110P can be processed at that condition, while a high-crystallinity PPS-GF grade may demand 135–150 °C to achieve acceptable crystallinity and dimensional stability. In such applications, the PBT phase remains the sacrificial phase under severe hydrolytic attack; if the component must withstand continuous exposure to boiling water at 140 °C for more than 1000 h, a fully PPS or high-temperature polyamide material may be required instead.
Relative to conventional PBT-GF30, AP-2110P shifts the dimensional stability window upward. The PPS phase increases heat deflection temperature under 1.80 MPa by approximately 20–40 °C and reduces moisture uptake under ISO 62. Relative to PPS-GF30, AP-2110P reduces the required melt and mold temperatures, improves impact toughness, and lowers material cost but sacrifices continuous-use thermal-oxidative resistance and high-temperature chemical resistance. Compared with unreinforced PBT/PPS blends, the glass fiber in AP-2110P increases flexural modulus and creep resistance under load; the trade-off is lower ultimate elongation and greater shrinkage anisotropy between flow and transverse directions. In thin-wall connector applications with wall sections of 0.4–0.8 mm, this anisotropy is managed by gating at the article perimeter and by specifying mold shrinkage values under ISO 294-4 after a 24 h post-mold stabilization period.
Because PBT/PPS/GF compounds are semi-crystalline and glass-fiber-filled, their reported mechanical properties depend strongly on specimen type, mold temperature, and moisture state. The comparison in the table below is a class-level summary for commercial glass-reinforced PBT/PPS alloys, PBT-GF30, and PPS-GF30; the values are not certified values for AP-2110P and must be replaced with the manufacturer’s certificate data in design calculations. Testing is performed after conditioning under 23 °C and 50% relative humidity for at least 88 h unless otherwise stated. For cross-reference, U.S. specifications often report tensile strength under ASTM D638-14, but values are not identical to ISO 527-2 because of different specimen geometry and strain rate.
| Property | PBT/PPS/GF class | PBT-GF30 | PPS-GF30 | Test basis |
|---|---|---|---|---|
| Density | 1.55–1.68 g/cm³ | 1.50–1.60 g/cm³ | 1.70–1.80 g/cm³ | ISO 1183 |
| Tensile strength at break | 120–150 MPa | 110–140 MPa | 140–170 MPa | ISO 527-2 |
| Flexural modulus | 10–14 GPa | 8–10 GPa | 13–16 GPa | ISO 178 |
| Heat deflection temperature at 1.80 MPa | 220–250 °C | 195–210 °C | 260–275 °C | ISO 75-1/-2 |
| Water absorption 24 h | <0.1% | 0.1–0.3% | <0.05% | ISO 62 |
| Mold shrinkage range | 0.1–1.0% | 0.2–1.2% | 0.2–1.0% | ISO 294-4 |
Compliance verification for AP-2110P is batch-specific. The matrix below identifies the standards and regulations commonly included in the material’s documentation; inclusion in this table does not replace the supplier’s declaration for a specific lot.
| Assessment | Standard or regulation | Typical required condition |
|---|---|---|
| Flammability classification | UL 94 | V-0 at 0.8 mm or as listed on UL Yellow Card; verify AP-2110P |
| Comparative tracking index | IEC 60112 | CTI 200 V or higher for electrical connector use; verify by test |
| Restriction of hazardous substances | 2011/65/EU | RoHS recast; no intentional Pb, Cd, Hg, Cr6+, PBB, PBDE except exemptions |
| REACH SVHC screening | Regulation (EC) No 1907/2006 | SVHC content below 0.1 wt% per article |
| Material marking | ISO 11469 | Marking for PBT/PPS glass-fiber designation as appropriate |
Operational boundaries for AP-2110P are defined by the PBT phase. The material is not recommended for continuous immersion in hot alkaline solutions above pH 9.0 at 80 °C, for high-temperature gear and bearing contacts exceeding 150 °C in continuous thermal-oxidative load, or for direct exposure to strong mineral acids at elevated temperature. When regrind is used above 20 wt%, lot-specific fiber length analysis and mold shrinkage capability studies are required before released production. Furthermore, addition of amine-based processing aids, color concentrates based on polyamide carriers, or flame retardant packages not pre-approved for PBT/PPS/GF alloys may destabilize the ester phase and should be validated by melt viscosity testing under ISO 1133-1:2022.