| HS Code | 527022 |
| Material Composition | PBT with 15% glass fiber |
| Density | 1.41 g/cm³ |
| Glass Fiber Content | 15% |
| Tensile Strength | 100 MPa |
| Tensile Elongation At Break | 3.0% |
| Flexural Modulus | 5500 MPa |
| Flexural Strength | 150 MPa |
| Charpy Notched Impact Strength | 5 kJ/m² |
| Heat Deflection Temperature At 1 82 Mpa | 200 °C |
| Melting Point | 225 °C |
| Water Absorption | 0.07% |
| Molding Shrinkage | 0.3–0.6% |
| Flammability Rating | HB |
As an accredited Mitsubishi Engineering Plastics Lumiloy® PBT+GF15% GP1000 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Packaged in 25 kg moisture-barrier bags, palletized: Mitsubishi Engineering Plastics Lumiloy® PBT+GF15% GP1000 resin, protected from moisture and contamination. |
| Container Loading (20′ FCL) | 20′ FCL container loading: palletized, shrink-wrapped bags of Mitsubishi Engineering Plastics Lumiloy® PBT+GF15% GP1000, evenly distributed and secured for export shipment. |
| Shipping | Mitsubishi Engineering Plastics Lumiloy® PBT+GF15% GP1000 is shipped as non-hazardous thermoplastic resin pellets, typically in sealed 25 kg moisture-barrier bags stacked on pallets. Keep dry and protect from heat, sunlight, and contamination during storage and transit. No special dangerous-goods classification applies under normal transport conditions. |
| Storage | Store **Lumiloy® PBT+GF15% GP1000** in original, sealed containers in a cool, dry, well-ventilated area, protected from sunlight, heat, moisture, and contamination. Keep away from oxidizers and ignition sources; avoid dust generation and static buildup. Maintain stable temperature, practice first-in/first-out, and follow the SDS. |
| Shelf Life | Typically 12 months when stored cool, dry, and in original unopened packaging; confirm with supplier. |
Competitive Mitsubishi Engineering Plastics Lumiloy® PBT+GF15% GP1000 prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Designed as a medium-stiffness PBT injection-moulding grade, Mitsubishi Engineering Plastics Lumiloy® PBT+GF15% GP1000 is a polybutylene terephthalate compound reinforced with 15% by weight chopped-strand E-glass fibre. The product is supplied in pellet form for conventional reciprocating-screw injection moulding and is positioned in the Lumiloy GP-series between unfilled PBT grades and higher glass-fibre grades such as GP2000 and GP3000. The material is used in multi-pin connectors, relay bobbins, power-tool housings, lamp sockets, small electric-motor brush holders, and flat insulator strips where a balance of rigidity, dimensional stability, and melt flow is required. Supplier-published typical values for dry-as-moulded specimens include a density of 1.31 g/cm³ by ISO 1183-1, tensile stress at break of 93 MPa by ISO 527-1/2, flexural modulus of 4,500 MPa by ISO 178, notched Charpy impact of 4.0 kJ/m² by ISO 179-1/1eA, and heat deflection temperature at 1.80 MPa of 195 °C by ISO 75-1/A. The melt volume-flow rate, measured at 250 °C under a 2.16 kg load by ISO 1133-1, is approximately 20 cm³/10 min. The grade is supplied according to EU RoHS 2011/65/EU and REACH SVHC declarations; current UL Yellow Card data should be verified for specific colour, thickness, and end-use electrical ratings.
| Property | Value | Standard |
|---|---|---|
| Density | 1.31 g/cm³ | ISO 1183-1 |
| Tensile stress at break | 93 MPa | ISO 527-1/2 |
| Tensile elongation at break | 3.5 % | ISO 527-1/2 |
| Flexural strength | 150 MPa | ISO 178 |
| Flexural modulus | 4,500 MPa | ISO 178 |
| Notched Charpy impact strength at 23 °C | 4.0 kJ/m² | ISO 179-1/1eA |
| Heat deflection temperature at 1.80 MPa | 195 °C | ISO 75-1/A |
| Melt volume-flow rate at 250 °C / 2.16 kg | 20 cm³/10 min | ISO 1133-1 |
| Mould shrinkage, flow direction | 0.6–1.0 % | ISO 294-4 |
Values in the table are typical engineering references, not batch-release specifications. Moulded-part properties depend on gate geometry, flow length, fibre orientation, weld-line position, and cooling-rate history. Tensile strength measured on plaques can differ by 10–15% between flow and cross-flow directions because short-glass fibres align preferentially with the local flow field.
At 15% glass-fibre loading, the material occupies a narrow processing-performance corridor between unfilled PBT and 30% glass-fibre PBT. Unfilled PBT typically exhibits mould shrinkage of 1.5–2.0% in the flow direction and a flexural modulus near 2,500 MPa. GP1000 reduces flow-direction shrinkage to 0.6–1.0% and raises flexural modulus to 4,500 MPa. Reinforcement also increases heat deflection temperature from approximately 58 °C to 195 °C at 1.80 MPa because the glass network suppresses creep under load. Moving from GP1000 to a 30% glass-fibre PBT raises flexural modulus to approximately 7,500 MPa and heat deflection temperature to 205 °C, but the higher fibre fraction reduces spiral-flow length by 20–30% and increases density to approximately 1.53 g/cm³. For moulders this changes gating decisions: high-glass grades may require wider edge gates or additional gates in flat rectangular connectors, whereas GP1000 can often be processed with a single submarine gate in parts up to 2 mm wall thickness.
Fibre orientation is the dominant source of mechanical anisotropy. When melt arrives through a single gate, glass fibres orient parallel to the local flow direction and produce higher tensile strength in that axis. A centrally gated flat part develops a radial orientation pattern and nonlinear shrinkage; mould shrinkage measured by ISO 294-4 can show differences of 0.2–0.5 percentage points between flow and transverse directions. GP1000 exhibits lower anisotropy than PBT+GF30 because the lower fibre volume fraction reduces fibre–fibre interaction and rotation resistance during fountain flow at the melt front. Weld-line tensile strength in GP1000 is generally 55–65% of parent tensile strength; in a 30% glass-fibre grade, weld-line strength can fall to 45–55% because few fibres cross the weld plane.
Production-scale experience in 16-cavity hot-runner connector moulds indicates that GP1000 fills 0.8 mm walls at 800–1,000 bar peak injection pressure using a 130 t clamp. A comparable GF30 grade can require 15–20% higher pressure and can generate core-pin deflection when unsupported pin length exceeds 8 times pin diameter. When flatness specification is 0.15 mm across a 60 mm span, GF30 parts may require post-moulding conditioning or jig cooling, whereas GP1000 parts can often be removed and measured without secondary correction. These moulding differences make GP1000 a candidate for thin-wall electrical components where flash, pin sweep, and dimensional repeatability are critical.
PBT is hydrolytically sensitive at melt temperature; water reacts with ester linkages and reduces molecular weight. Supplier handling guidance for GP1000 recommends pre-drying at 120 °C for 4 h in a desiccant-bed dehumidifying hopper with a dew point of -40 °C or lower. Residual moisture should be verified below 0.02% by ISO 15512:2019 or an equivalent Karl Fischer procedure. At 0.05% residual moisture, a reduction in notched Charpy impact of 15–20% and tensile strength of 5–10% is observed in PBT compounds because hydrolytic chain scission preferentially attacks the amorphous tie-chain population that governs fracture resistance. Regrind exposed to 55% relative humidity can rise from 0.02% to 0.08% within 1 h; therefore regrind should be dried with virgin material and limited to a maximum of 20% by weight when impact-sensitive parts are moulded.
Barrel temperature should not exceed 270 °C. A melt temperature of 250–270 °C is suitable for GP1000; at the lower end, glass-fibre dispersion is adequate if back pressure is 0.3–0.5 MPa and screw speed is 80–150 rpm. At 280 °C, PBT degradation accelerates and discoloration increases; residence time at melt temperature must not exceed 8 min in conventional screw-and-barrel systems. In hot-runner systems with manifold volume greater than 1.5 times shot volume, manifold temperature should be reduced to 240–250 °C and valve-gate sequencing should be used to eliminate stagnant melt regions. Moulders should also confirm that screw recovery time does not exceed cooling time; an oversized barrel can extend residence time and reduce notched Charpy impact despite correct barrel temperatures.
Table 2 compares representative values for GP1000, unfilled PBT, and a 30% glass-fibre PBT. The values are derived from supplier technical literature and moulded plaque data; actual results shift with colour, thickness, gate geometry, and packing conditions.
| Property | GP1000 PBT+GF15% | Unfilled PBT | PBT+GF30 |
|---|---|---|---|
| Tensile stress at break, ISO 527-1/2 | 93 MPa | 55 MPa | 120 MPa |
| Flexural modulus, ISO 178 | 4,500 MPa | 2,500 MPa | 7,500 MPa |
| Notched Charpy impact at 23 °C, ISO 179-1/1eA | 4.0 kJ/m² | 3.0 kJ/m² | 6.0 kJ/m² |
| Heat deflection temperature at 1.80 MPa, ISO 75-1/A | 195 °C | 58 °C | 205 °C |
| Mould shrinkage, flow direction, ISO 294-4 | 0.6–1.0 % | 1.5–2.0 % | 0.3–0.6 % |
The difference between GP1000 and PBT+GF30 is not only stiffness and impact. The 15% glass-fibre grade retains a smoother melt-front appearance and lower melt pressure in thin sections, while still reducing shrinkage by roughly 40–60% relative to unfilled PBT. Conversely, the 30% glass-fibre grade is preferable when maximum load-bearing capacity and creep resistance are required, at the cost of higher tool wear from glass abrasion, higher injection pressure, and greater warpage sensitivity in unbalanced moulds.
For flat connector insulators moulded in PBT+GF30, saddle warpage often arises because the higher fibre fraction creates a stronger orientation-stress gradient through thickness. With GP1000, the 15% fibre loading lowers orientation stress, but packing pressure remains critical: a packing-pressure reduction from 60 to 30 MPa can increase shrinkage by 0.2–0.4 percentage points and open the dimensional tolerance window. For parts with thickness below 1 mm, gate freeze time should be confirmed by short-shot studies; if gate diameter is below 0.8 mm, premature gate freeze can cause underpacking, increased moulded-in stress, and higher warpage after ejection.
Chemical resistance data for GP1000 follow general PBT behaviour: the grade withstands automotive fuels, aliphatic hydrocarbons, mineral oils, and many common solvents at ambient temperature, but is not recommended for continuous immersion in hot water above 80 °C, strong alkaline solutions, or steam sterilisation above 100 °C because PBT hydrolysis is autocatalytic and glass-fibre wicking accelerates fluid ingress. Published data for this specific configuration is limited, and the supplier’s chemical-resistance chart for PBT should be consulted for each contact fluid. For applications requiring a UL 94 V-0 classification at 0.75 mm, flame-retarded Lumiloy grades or a glass-filled PBT with halogenated or red-phosphorus flame retardant must be substituted; GP1000 is typically supplied as a non-flame-retarded grade. Electrical tracking index should be verified against the current UL Yellow Card and IEC 60112 data for the specific colour and thickness because glass-fibre content can reduce comparative tracking index in humid service environments.