| HS Code | 187883 |
| Density | 1.53 g/cm³ |
| Glassfibercontent | 30 % |
| Tensilestrength | 100 MPa |
| Tensileelongationatbreak | 2.0 % |
| Flexuralmodulus | 8,000 MPa |
| Flexuralstrength | 150 MPa |
| Notchedcharpyimpactstrength | 6 kJ/m² |
| Heatdeflectiontemperatureat1 82mpa | 200 °C |
| Heatdeflectiontemperatureat0 45mpa | 210 °C |
| Meltingpoint | 224 °C |
| Flameretardancy | UL 94 V-0 |
| Moldingshrinkageflow | 0.3–0.6 % |
| Moldingshrinkagecrossflow | 0.6–1.0 % |
| Waterabsorption24h | 0.06 % |
| Volumeresistivity | 1 × 10^16 Ω·cm |
| Dielectricstrength | 20 kV/mm |
| Arcresistance | 120 s |
As an accredited Mitsubishi Chemical Novaduran™ PBT+GF30% LW-V0 5710GN1-30 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Mitsubishi Chemical Novaduran™ PBT+GF30% LW-V0 5710GN1-30 is supplied in 25 kg moisture-resistant, sealed bags for safe storage and transport. |
| Container Loading (20′ FCL) | Container Loading (20′ FCL): Palletized 25kg bags of Mitsubishi Chemical Novaduran™ PBT+GF30% LW-V0 5710GN1-30, shrink-wrapped and secured for ocean transport. |
| Shipping | Mitsubishi Chemical Novaduran™ PBT+GF30% LW-V0 5710GN1-30 is shipped as moisture-sensitive thermoplastic pellets in sealed, labeled moisture-barrier bags or drums. Transport under dry, ambient conditions, away from direct sunlight and ignition sources. Normally not classified as dangerous goods; follow the SDS and local regulations. |
| Storage | Store in a cool, dry, well-ventilated warehouse away from direct sunlight, heat sources, open flames, moisture, and oxidizing agents. Keep original packaging sealed and pallets off the floor to prevent moisture absorption and contamination. Use first-in, first-out stock rotation; avoid prolonged storage in humid or high-temperature conditions. |
| Shelf Life | Typical shelf life is 12 months when stored dry in original sealed packaging at temperatures below 30°C. |
Competitive Mitsubishi Chemical Novaduran™ PBT+GF30% LW-V0 5710GN1-30 prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
The full designation Mitsubishi Chemical Novaduran™ PBT+GF30% LW-V0 5710GN1-30 identifies a polybutylene terephthalate compound reinforced with 30% glass fibre by mass, carrying a low-warpage additive package and a flame-retardant system that achieves UL 94 V-0 classification at a specified minimum wall thickness. The grade is delivered as cylindrical pellets and is intended for injection moulding of dimensionally stable electrical and electronic housings, connectors, relay bases, and structural power-distribution components. The suffix LW-V0 distinguishes the material from conventional glass-filled PBT grades by targeting anisotropic mould shrinkage reduction rather than simply increasing filler level. Published manufacturer datasheets place the material in the general density range of 1.65 g/cm³ to 1.70 g/cm³ under ISO 1183 and list a UL 94 flammability rating of V-0 at 0.75 mm test thickness, although the current certificate for the specific production plant should be confirmed because flame-retardant formulations are periodically adjusted to regional regulatory requirements.
Prior to melt processing, the compound requires closed-loop desiccant drying at 120°C to 140°C for 4 h to 6 h. The residual moisture content must be held below 0.02% because the PBT ester linkage is hydrolysis-sensitive. A dehumidified-air dryer with dew point at or below -40°C is preferable to hot-air ovens. Barrel temperature settings are typically profiled between 250°C and 270°C from rear to nozzle; excursions above 280°C accelerate decomposition of the flame-retardant system and produce surface deposits, while temperatures below 245°C reduce glass-fibre dispersion and cause non-uniform mould fill. The processing window is therefore narrow, and thermal control should be verified at the nozzle with a calibrated probe rather than inferred from setpoint. A three-zone general-purpose screw with L/D in the 20:1 to 22:1 range and compression ratio near 2.0:1 to 2.5:1 is commonly used. Back pressure should remain between 3 MPa and 7 MPa; higher back pressure raises melt temperature and may degrade the FR package. Screw rotation speed should be adjusted so that residence time at full melt temperature does not exceed 10 min; longer residence time is associated with black speck formation and a decline in UL 94 performance. Mould temperature is normally controlled between 60°C and 100°C, depending on wall thickness and dimensional tolerance. Hot-runner systems require external heating and smooth, polished melt channels because halogenated decomposition products can attack unprotected steel surfaces. On production lines, injection pressure at the transfer point is often in the 80 MPa to 120 MPa range for connectors with wall sections of 0.8 mm to 1.5 mm; shot masses outside the validated range should be checked before adjusting melt temperature. The grade should not be purged with polyolefin after shutdown; a recognised purging compound with adequate thermal stability above 270°C is recommended.
No single mechanical value defines the product; specification requires simultaneous review of short-term strength, impact resistance, and heat-deflection response. Under ISO 527-1/2, 30% glass-filled flame-retardant PBT of this class typically exhibits tensile strength in the 115 MPa to 135 MPa range and tensile modulus from 9,000 MPa to 11,500 MPa. Elongation at break is usually 2% to 3%, reflecting the brittle response introduced by both glass fibre and the FR filler. Flexural modulus under ISO 178 commonly falls between 9,500 MPa and 11,500 MPa, while notched Charpy impact at 23°C under ISO 179-1/1eA is generally 5 kJ/m² to 8 kJ/m². These values should be interpreted as typical production ranges for the LW-V0 product class, not guaranteed lot minima; the current manufacturer datasheet and lot certificate for grade 5710GN1-30 take precedence. The heat-deflection temperature under 1.80 MPa load is typically above 200°C when measured according to ISO 75-1/2, but the part should not be loaded continuously near this value because PBT matrices lose stiffness through creep at elevated temperature. Melt volume-flow rate at 250°C and 2.16 kg load is commonly in the 15 cm³/10 min to 25 cm³/10 min range under ISO 1133-1:2022. The following table summarises the main property window used for initial design review.
| Property | Test method | Typical design range |
|---|---|---|
| Density | ISO 1183 | 1.65–1.70 g/cm³ |
| Tensile strength at 23°C | ISO 527-1/2 | 115–135 MPa |
| Tensile modulus | ISO 527-1/2 | 9,000–11,500 MPa |
| Flexural modulus | ISO 178 | 9,500–11,500 MPa |
| Notched Charpy impact at 23°C | ISO 179-1/1eA | 5–8 kJ/m² |
| HDT at 1.80 MPa | ISO 75-1/2 | 200–215 °C |
| Melt volume-flow rate | ISO 1133-1:2022 | 15–25 cm³/10 min at 250°C, 2.16 kg |
| UL 94 flammability | UL 94 | V-0 at 0.75 mm |
Warpage in glass-fibre-reinforced semicrystalline polymers is caused mainly by anisotropic shrinkage between flow and transverse directions. In conventional 30% glass-filled PBT, glass fibres orient along the melt-flow path and restrict shrinkage in that direction, while transverse shrinkage remains higher; the mismatch generates internal stress and bowing in flat parts. The LW-V0 formulation interrupts this anisotropy through filler morphology adjustments and may show flow-direction mould shrinkage near 0.2% to 0.4% and transverse shrinkage near 0.4% to 0.6% under ISO 294-4. Direct comparison against a non-LW GF30 V-0 grade should be performed on the same tool because gate location, wall-thickness transitions, and packing pressure modify the measured delta. For flat housings with weld lines, the reduced differential shrinkage is an advantage in planarity; however, the low-warpage package can increase stiffness locally at knit lines, and a short-shot study is recommended before production release.
Primary use is in injection-moulded electrical and electronic enclosures where UL 94 V-0 is a condition of market access. The combination of 30% glass reinforcement and V-0 flame retardancy supports connector housings, headers, sockets, relay bases, terminal blocks, circuit-breaker internal frames, and power-supply enclosures. In electric vehicle charging infrastructure, the grade is evaluated for connector bodies and holster housings where dimensional stability across temperature cycling and low flammability are required. Field experience on production moulding machines indicates that clamp-force capacity must be selected for the filled grade; a connector housing with projected area of 150 cm² may require clamp force above 120 t when mould filling is completed at 100 MPa packing pressure. Short-shot tendencies are more common in thin-wall sections below 0.8 mm because the glass-fibre network increases viscosity relative to unfilled PBT; injection speed should be maintained rather than relying on melt-temperature increases above 270°C. Part design should avoid living hinges, large undercuts, and threaded metal inserts without preheating, because the low elongation at break reduces post-mould deflection capacity. Electrical property data should be obtained from the current datasheet; glass fibre and FR fillers generally reduce dielectric strength relative to unfilled PBT. Under IEC 60243-1, short-term dielectric strength for 30% GF FR PBT is usually 18 kV/mm to 24 kV/mm on 2 mm plaques, while volume resistivity at 500 V is typically above 1 × 10¹³ Ω·m under IEC 62631-3-1. The comparative tracking index under IEC 60112 may fall in the 200 V to 250 V range, which is lower than many unfilled PBT grades; therefore creepage distances must be designed to the CTI value of the final compound, not to the base polymer.
The substitution is not always drop-in. Compared with a standard 30% glass-filled V-0 PBT, the low-warpage formulation changes pressure-dependent shrinkage behaviour and can alter the dimensional output of the same tool. Mould cavities originally sized for a non-LW grade may produce parts at the high end of tolerance if the LW-V0 grade shrinks less in the transverse direction; tool adjustment or packing-pressure profiling is needed. Weld-line strength is a second variable: low-warpage filler packages and glass-fibre orientation at meeting fronts can reduce elongation at break at knit lines by a measurable margin. Prototype trials should include tensile tests across weld lines using ISO 527-1/2 specimens cut from production parts or edge-gated plaques. Compared with unfilled PBT, the 5710GN1-30 grade raises tensile modulus by a factor of approximately 4 and reduces elongation at break from above 20% to below 5%, so snap-fit hooks and press-fit pins designed for unfilled PBT require redesign. Compared with a mineral-filled low-warpage PBT, the 30% glass grade provides higher modulus and better dimensional stability under load but lower surface gloss and higher notch sensitivity. The FR system also reduces comparative tracking index relative to non-FR PBT; electrical creepage and clearance distances should be revalidated to the final part standard, not the raw material property alone.
Compliance is documented at the substance and compound level. The grade is normally supplied with statements covering RoHS Directive 2011/65/EU and its delegated directives, REACH SVHC status, and absence of polybrominated biphenyls and polybrominated diphenyl ethers under relevant regional regulations. The following matrix summarises the typical documentation set associated with the compound; each item must be confirmed against the current supplier certificate because production site and regional formulation may vary.
| Requirement | Reference standard/regulation | Typical status for the LW-V0 grade |
|---|---|---|
| UL flammability classification | UL 94 | V-0 at 0.75 mm |
| RoHS hazardous substances | Directive 2011/65/EU | Compliant per supplier certificate |
| REACH SVHC | Regulation (EC) 1907/2006 | No SVHC above reporting threshold per current statement |
| Brominated dioxins/furans | Regional waste and electronics rules | Not intentionally added; supply-chain confirmation required |
| Mould shrinkage measurement | ISO 294-4 | Low differential shrinkage vs standard GF30 V-0 |
As a PBT compound, the ester backbone is subject to hydrolytic chain scission when wet. Water absorption under ISO 62 after 24 h at 23°C is commonly below 0.1%, but saturated absorption can exceed 0.4% after prolonged immersion. Continuous exposure to water or humid air above 85°C is not recommended because tensile strength and impact resistance decline as molecular weight drops. For outdoor electrical enclosures, UV exposure can cause surface chalking; the grade is not a weatherable polyester, and a suitable coating or UV-stabilised grade is preferred when direct sunlight is part of the service environment. Alkaline cleaning agents above pH 10 and concentrated strong acids at elevated temperature can attack the PBT matrix; compatibility testing should follow ISO 22088 or ISO 175 as applicable. The flame-retardant package can interact with metal inserts and electrical contacts when condensation films are present, so protective coatings on copper alloys are often specified in humid applications. These limitations do not reduce the grade’s suitability for dry interior electrical housings; they define the boundary between intermittent condensation service and immersion service. The compound should not be blended with amine-based additives or recycled PBT of unknown flame-retardant chemistry because additive interactions may shift UL 94 performance.