| HS Code | 501080 |
| Product Name | Mitsubishi Chemical Novaduran™ PBT+GF30%-Hydrolytic GTS-530 |
| Polymer Type | Polybutylene terephthalate (PBT) |
| Reinforcement | 30% glass fiber |
| Hydrolysis Resistance | Hydrolytically stabilized / hydrolysis-resistant |
| Molding Shrinkage Percent | 0.3-0.7 |
| Volume Resistivity Ohm Cm | 1E16 |
| Flammability Ul94 | HB |
As an accredited Mitsubishi Chemical Novaduran™ PBT+GF30%-Hydrolytic GTS-530 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Supplied in 25 kg moisture-resistant, palletized paper bags with clear product identification labels. |
| Container Loading (20′ FCL) | Container loading (20′ FCL) for Mitsubishi Chemical Novaduran™ PBT+GF30%-Hydrolytic GTS-530: palletized 25 kg bags, evenly distributed, braced and secured for ocean freight. |
| Shipping | Shipping description: Mitsubishi Chemical Novaduran™ PBT+GF30%-Hydrolytic GTS-530, hydrolysis-resistant, 30% glass-fiber reinforced PBT pellets, in sealed moisture-barrier bags/containers. Transport in cool, dry, ventilated conditions, away from heat, moisture, sunlight, and contamination. Stack securely; protect packaging from damage. Typically non-hazardous thermoplastic; follow SDS and local regulations. |
| Storage | Store Mitsubishi Chemical Novaduran™ PBT+GF30%-Hydrolytic GTS-530 in a cool, dry, well-ventilated area away from direct sunlight, heat sources, and moisture. Keep containers tightly closed and protect from contamination, acids, alkalis, and oxidizing agents. Avoid humid conditions, use dry handling practices, and follow manufacturer/SDS temperature and shelf-life recommendations. |
| Shelf Life | Shelf life: 12 months from manufacture when stored unopened in original packaging, dry, cool, and protected from moisture. |
Competitive Mitsubishi Chemical Novaduran™ PBT+GF30%-Hydrolytic GTS-530 prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
The product identified as Mitsubishi Chemical Novaduran™ PBT+GF30%-Hydrolytic GTS-530 is a hydrolytically stabilized polybutylene terephthalate injection-molding compound reinforced with nominally 30% by weight short glass fiber. The grade is positioned for hot-moisture environments where conventional PBT-GF30 compounds exhibit autocatalytic ester hydrolysis at fiber-matrix interfaces and at surface microcracks after prolonged exposure to water, coolant, or humid air. The base semicrystalline PBT matrix has a melting range of approximately 220–225°C and a glass transition near 45–60°C; glass reinforcement raises modulus, tensile strength, and heat distortion temperature relative to unfilled PBT. The commercial designation GTS-530 does not appear with complete property disclosure in all public cross-reference databases, so the numerical ranges in this document are representative for a hydrolysis-resistant 30% glass-fiber-reinforced PBT and should be checked against the manufacturer’s certificate of analysis, technical data sheet, or UL Yellow Card. The grade differs from standard PBT-GF30 primarily through the hydrolytic stabilization package, not through fiber loading or base resin chemistry.
Published data for this specific configuration is limited, but the function of a hydrolytic stabilizer in PBT is well characterized. Polybutylene terephthalate contains ester linkages that are susceptible to chain scission in the presence of water and heat. The degradation mechanism is acid-catalyzed: each hydrolytic cleavage generates a carboxylic acid end group, which further accelerates ester hydrolysis. A hydrolysis-resistant grade such as GTS-530 is formulated to reduce the available carboxylic acid end-group concentration and to interrupt the autocatalytic degradation loop through acid scavenging, chain extension, or end-group capping. In standard PBT-GF30, long-term strength retention in pressurized hot coolant can decline substantially because moisture attacks the fiber sizing and the matrix simultaneously, causing interfacial debonding and surface microcracking. Stabilized grades are intended to retain a higher fraction of ultimate tensile stress measured according to ISO 527-2:2012 and a higher fraction of flexural modulus measured according to ISO 178:2019 after aging in hot water/glycol mixtures. Notched Charpy impact energy under ISO 179-1:2023, condition 1eA, is used as an indirect indicator of interfacial durability because impact strength is sensitive to loss of fiber-matrix adhesion.
| Property | Standard | Unfilled PBT | Standard PBT-GF30 | Hydrolysis-resistant PBT-GF30, GTS-530 representative range |
|---|---|---|---|---|
| Density | ISO 1183-1:2019 | 1.30–1.32 g/cm³ | 1.50–1.54 g/cm³ | 1.51–1.55 g/cm³ |
| Tensile stress at break, dry as molded | ISO 527-2:2012 | 50–60 MPa | 130–145 MPa | 125–140 MPa |
| Flexural modulus, dry as molded | ISO 178:2019 | 2.3–2.5 GPa | 8.5–9.5 GPa | 8.0–9.0 GPa |
| Notched Charpy impact, 23°C | ISO 179-1:2023, 1eA | 3–5 kJ/m² | 8–12 kJ/m² | 7–10 kJ/m² |
| Heat distortion temperature, 1.80 MPa | ISO 75-2:2013 | 50–60°C | 205–215°C | 200–210°C |
| Mold shrinkage, parallel / normal | ISO 294-4:2018 | 1.5–2.0% / 1.5–2.0% | 0.2–0.4% / 0.7–1.0% | 0.2–0.5% / 0.7–1.0% |
The ranges in the third column are compiled from hydrolysis-resistant PBT-GF30 grades and should not be read as specification limits for GTS-530 unless confirmed by Mitsubishi Chemical. The primary difference in aged property retention, rather than dry-as-molded mechanical values, is the technical justification for selecting this grade.
Hydrolytically stabilized PBT-GF30 retains the processing profile of semi-crystalline PBT but requires stricter moisture control than many unfilled aromatic polyesters because the stabilizer does not eliminate the need for pre-drying. Trapped moisture at melt temperature causes hydrolytic chain scission during the molding cycle itself and can produce splay, reduced impact strength, and surface defects. The compound should be dried in a desiccant dryer to a residual moisture target of ≤0.02 wt%, preferably ≤0.01 wt%, before melt processing. A drying temperature of 120°C for 4–6 h at a dew point of −40°C is typical for PBT-GF30 hydrolysis-resistant grades. Extended exposure at 120°C should be limited to avoid oxidative discoloration and loss of stabilizer activity. Melt temperature measured at the nozzle should be kept within 250–270°C; a mold temperature of 80–120°C is necessary to achieve sufficient crystallization and to minimize post-mold shrinkage. Barrel residence time should not exceed 8–10 min at maximum melt temperature because excessive residence accelerates both thermal degradation and residual-moisture hydrolysis. Processing on a general-purpose single-stage screw with an L/D ratio of 20:1 to 24:1 is common. A low-compression screw with a gradual transition zone and a free-flow check ring reduces glass-fiber breakage and melt-temperature overshoot. Injection speed should be moderate to high to maintain fiber length, but excessive shear can reduce average fiber length and lower tensile modulus. Packing pressure and hold time should be set against gate freeze; typical gate diameters for PBT-GF30 are at least 0.8–1.0 mm for small components and 1.5–2.0 mm for thick-walled parts. Hot-runner and manifold channels must be free of dead spots because stagnating melt can degrade and contaminate subsequent shots.
Production-scale failure modes reported for glass-reinforced PBT compounds include splay from residual moisture above 0.03 wt%, gate blush from insufficient hot-tip temperature, jetting from undersized gates, and warpage caused by differential fiber orientation. These issues are not unique to GTS-530 but are amplified by the low melt-viscosity character of PBT and the anisotropy of short glass fiber. Mold-flow simulation using filling and warpage modules is recommended when gate count, gate location, and wall thickness are changed from the prototype tool to the production tool.
Applications that require continuous exposure to engine coolant, hot water, or humid underhood air are the primary usage domain for GTS-530. Components in this category include thermostat housings, water pump impellers, coolant control valves, degas tanks, temperature sensor housings, coolant connectors, and electronic throttle body components. In these systems, the material contacts water/glycol mixtures at operating temperatures often between 90°C and 130°C and pressure cycling from 0.1 bar to 2.0 bar. Standard PBT-GF30 loses tensile strength faster under these conditions because the ester bonds are hydrolytically cleaved and because the glass-fiber sizing can be attacked by absorbed water. The GTS-530 hydrolytic stabilization package is intended to extend the time to 50% ultimate tensile stress retention, as measured after immersion in a 50:50 water/ethylene glycol mixture at 120°C under sealed pressure-vessel conditions. The grade is not a substitute for PPS or PPA in sustained service above 150°C, nor is it suitable for strong alkaline coolant concentrates with pH above 9.5–10.0 without explicit validation. It is also not recommended for direct contact with undiluted glycol above the boiling point of the coolant mixture unless validated under SAE J2412 or internal OEM endurance protocols.
Compared with standard Novaduran PBT-GF30 grades, GTS-530 differs primarily in the additive package rather than fiber loading or base resin. The hydrolytic stabilizer is not a flame-retardant system; therefore UL 94 classification is typically the same as a non-flame-retarded PBT-GF30 grade, commonly HB at 1.5 mm unless a specific FR grade is selected. The stabilizer can slightly alter melt viscosity and elongation at break, so processing parameters established for a non-stabilized PBT-GF30 should not be transferred without re-qualification. Compared with low-warpage PBT-GF30 grades that use mineral or glass-flake fillers, GTS-530 retains the mechanical anisotropy associated with short glass fiber; shrinkage parallel and perpendicular to flow direction differs, so gate placement and part geometry drive warpage more strongly. Compared with hydrolysis-resistant PBT grades without glass fiber, GTS-530 offers higher flexural modulus and heat distortion temperature but lower notched impact resistance and higher density. Compared with hydrolysis-resistant PBT/mineral blends, GTS-530 has higher tensile strength and better surface appearance but higher mold shrinkage anisotropy.
| Test or requirement | Standard or regulation | Condition | Technical purpose |
|---|---|---|---|
| Dry-as-molded tensile properties | ISO 527-2:2012 | 5 mm/min, Type 1A, 23°C | Baseline mechanical characterization |
| Flexural modulus | ISO 178:2019 | 2 mm/min, 80 mm × 10 mm × 4 mm | Stiffness under bending |
| Notched Charpy impact | ISO 179-1:2023 | 1eA, 23°C, notch radius 0.25 mm | Impact sensitivity and fiber-matrix adhesion |
| Heat distortion temperature | ISO 75-2:2013 | 1.80 MPa, flatwise | Short-term thermal resistance |
| Density | ISO 1183-1:2019 | Water immersion, 23°C | Material density for part mass control |
| Mold shrinkage | ISO 294-4:2018 | 60 mm × 60 mm × 2 mm plaque | Molding tolerance prediction |
| Flammability class | UL 94 | 0.8 mm or 1.5 mm thickness | Electrical enclosure use |
| SVHC compliance | REACH Regulation (EC) No 1907/2006 | Article 33 substance list | Regulatory compliance |
| Hazardous substance restriction | RoHS 2011/65/EU | 0.1 wt% per homogeneous material for lead, mercury, hexavalent chromium, PBDEs, PBBs; 0.01 wt% for cadmium | Electrical and electronic equipment compliance |
Selection of GTS-530 should be based on the hydrolytic aging requirement rather than dry-as-molded strength alone. If the component operates below 60°C in dry air, a standard PBT-GF30 may provide a more cost-efficient property set. If the component operates in hot coolant or saturated underhood air, the stabilizing additive package is the governing design variable. Qualification should include not only initial mechanical properties but also property retention after coolant immersion, thermal cycling, and pressure fluctuation representative of the final assembly. The exact retention values for Mitsubishi Chemical Novaduran™ PBT+GF30%-Hydrolytic GTS-530 must be obtained from the current technical data sheet because the published data for this specific configuration is limited.