| HS Code | 579527 |
| Polymer Type | Polyethylene, Linear Low Density |
| Density | 0.935 g/cm³ |
| Melt Index | 3.5 g/10 min |
| Tensile Strength At Yield | 14 MPa |
| Tensile Strength At Break | 20 MPa |
| Elongation At Break | 700% |
| Flexural Modulus | 552 MPa |
| Hardness Shore D | 55 |
| Vicat Softening Temperature | 107 °C |
| Melting Temperature | 124 °C |
| Thermal Conductivity | 0.35 W/m·K |
| Specific Heat Capacity | 2.3 J/g·°C |
| Coefficient Of Linear Thermal Expansion | 1.5E-4 1/°C |
| Environmental Stress Crack Resistance | >1000 h |
| Color | Green |
| Uv Stabilizer | Present |
As an accredited LyondellBasell Icorene 3545 GRN 6229 Polyethylene, Linear Low Density factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Standard packaging: 25 kg polyethylene-lined bags, 40 bags per 1,000 kg pallet; also available in 1,000 kg bulk bags or bulk trucks. |
| Container Loading (20′ FCL) | A 20′ FCL container loaded with LyondellBasell Icorene 3545 GRN 6229 linear low-density polyethylene resin, securely stowed for transport. |
| Shipping | LyondellBasell Icorene 3545 GRN 6229 Polyethylene, Linear Low Density is a non-hazardous, solid plastic resin typically shipped in 25 kg bags, octabins, or bulk trucks/containers. Store in cool, dry conditions away from sunlight, moisture, and contaminants. No special transport classification; handle as ordinary polymer resin. |
| Storage | Store LyondellBasell Icorene 3545 GRN 6229 Polyethylene, Linear Low Density indoors at ambient temperature in a cool, dry, well-ventilated area away from direct sunlight, heat, sparks, and flames. Keep containers tightly closed to prevent moisture, dust, and contamination. Avoid strong oxidizing agents. Maintain clean, segregated storage; use first-in, first-out inventory. Protect from physical damage and excessive stacking. Follow local regulations and SDS recommendations. |
| Shelf Life | Shelf life: Two years from production date when stored unopened in original packaging, dry, below 50°C, away from direct sunlight. |
LyondellBasell Icorene 3545 GRN 6229 enters the rotomolding supply chain as a linear low-density polyethylene powder in precolored green form. Closed-carousel or shuttle rotational molding machines with biaxial mold rotation are used to convert the powder into chemical containment vessels where a pinhole-free inner wall and stress-crack resistance under continuous liquid contact are non-negotiable. The mold charging weight is calculated from the part surface area, target wall thickness between 4 mm and 25 mm, and the melt density of the grade; oven set temperatures are normally 260°C–300°C while peak internal air temperature is controlled between 190°C and 220°C. A powder fraction passing a 35 mesh (500 µm) screen with a bulk density commonly between 0.32 g/cm³ and 0.42 g/cm³ measured by ASTM D1895 supports uniform wet-out in deep draw corners, while coarse fractions above 500 µm can remain as partially fused particles on the inside wall and create pinholes at the parting line. If the peak internal air temperature remains below 190°C, the resin retains a granular structure in narrow ribs and around insert bosses; if it exceeds 250°C, thermo-oxidative chain scission reduces environmental stress crack resistance measured by ASTM D1693 and produces brittle failure in the finished tank. Cooling must be staged from forced air to water mist only after the molten wall drops below 110°C; quenching directly from oven temperature introduces residual stress at weld lines and increases warpage in flat tank walls. For hazardous-liquid transport, the molded container falls under UN Model Regulations design-type testing and must pass leakproofness, hydrostatic pressure, and drop tests before a UN mark is assigned. Inserts and nozzles should be joined by heated-tool butt welding or hot gas extrusion welding using a rod generated from the same resin family; a poorly welded joint becomes a notch and initiates stress crack growth under service stress. Concentrated oxidizing acids, halogenated solvents, and low-boiling aromatic hydrocarbons are not suitable for continuous storage above 40°C; site-specific chemical resistance trials should be conducted before the tank is placed in service. Typical end products include double-wall secondary containment tanks, conical-bottom mixing vessels, and closed-head agricultural chemical containers.
Rotational molding of livestock watering troughs, hydroponic nutrient reservoirs, and nursery tables uses wall sections between 3 mm and 6 mm, which shifts the process boundary toward the low end of the sintering window. At a peak internal air temperature of 190°C–205°C, the LLDPE powder coalesces into a continuous film but may not fully collapse air bubbles trapped at corner weld lines; at 210°C–220°C, bubble collapse is more complete, but extended residence at this temperature can surface-oxidize the outer wall and shift the green color toward a yellowed appearance. Two-stage heating is therefore used on elongated trough molds: an initial oven phase at 280°C–300°C drives the internal air temperature to the target quickly, followed by a soak at 240°C–260°C to consolidate the structure without exceeding 220°C. Rotation ratio on large trough molds is not fixed; a major-to-minor axis ratio of 2:1 is common for long sidewall-dominated geometries, but deep end caps may require a supplementary dwell on the minor axis to avoid thin-out. If the grade is not already supplied with a weather-resistant package sufficient for the service life, a hindered amine light stabilizer masterbatch is dry-blended at 2–4 wt% in a high-intensity paddle mixer at 60–80 rpm for 8–12 min before the powder is charged. Dispersion defects appear as streaking on flat sidewalls and are quantified by color measurement under CIE Lab conditions or by accelerated weathering per ASTM G154. In use, trace fertilizers, iron sulfate supplements, and chlorinated water increase the rate of environmental stress cracking; welded corners should be evaluated by ASTM D5397 or ASTM D1693 after production to confirm that local stress concentrations do not produce premature fracture. Published data for this specific green color-adjusted formulation is limited; the optimum peak internal air temperature should be fixed from first-shot trials on the actual mold rather than transferred from unpigmented LLDPE rotomolding grades. Products include single- and double-walled livestock water troughs, hydroponic trays, and nursery bench liners.
In thin-shell kayak hulls and paddleboard bodies, the main defect is not chemical attack but cold-flow weld formation in long tapered bow sections and around recessed carry handles. The wall thickness in these areas can drop to 4 mm–6 mm, and the shot weight must be held within a narrow tolerance because an excess produces inner-wall sagging while a shortage produces holes at the stern tip. A higher minor-axis rotation speed relative to the major axis is often required to force powder into narrow ends; however, too high a minor-axis speed can starve the center section and create a longitudinal thinning band. Peak internal air temperature is kept between 195°C and 215°C, with oven set temperatures of 270°C–290°C. Aluminum molds with a vapor-honed or grained surface are preferred for kayak shells because the texture masks flow lines and reduces the visual impact of minor color variation in GRN 6229. Before the shell is considered marine-grade, tensile properties are measured on molded test plaques per ASTM D638, and low-temperature impact is assessed by ASTM D256 or instrumented puncture per ISO 6603-2 at -20°C. For buoyancy modules and dock floats, the rotationally molded LLDPE outer shell is filled with a two-part closed-cell polyurethane foam having a free-rise density of 32–48 kg/m³; the foam exotherm can exceed 120°C, so the shell must be cooled below 50°C before foam injection to prevent outer surface distortion. Water absorption of the shell material should be below 0.01% measured by ASTM D570; any higher value indicates through-wall porosity created by insufficient sintering. The product family includes sit-on-top kayak hulls, canoe float bags, and cylindrical dock pontoons.
Outdoor refuse containers, wheeled bin bodies, and municipal litter housings are frequently dry-blended with recycled LLDPE or HDPE to reduce material cost. At recycled content up to 20 wt%, rotational molding can still produce a cohesive wall if the recycled fraction is ground to pass a 35 mesh screen and its melt flow rate falls within ±30% of the virgin grade. Above 30 wt%, the viscosity mismatch between the two phases produces surface pitting, incomplete densification at rib intersections, and cold-flow weld lines that cannot be eliminated by increasing the peak internal air temperature alone. A pre-extrusion compounding step on a co-rotating twin-screw extruder with an L/D ratio of 44:1 and melt temperature below 220°C is then required to restore melt homogeneity and preserve environmental stress crack resistance. Because GRN 6229 is a precolored green powder, changes in recyclate addition also shift the final color; batch-to-batch color should be controlled under CIE Lab conditions with a ΔE tolerance of ≤1.5 relative to a retained standard, not merely by visual inspection. Drop impact resistance of refuse bodies is measured by ISO 6603-2 instrumented puncture at -20°C; rapid water-mist cooling immediately after oven removal can reduce cold impact by locking in residual stress at the base corners. Slow air cooling through the 60°C–80°C band allows stress relaxation but extends the cycle. For outdoor weatherability, a green colorant alone is not a reliable UV screen; if the article is specified for continuous exterior exposure, the formulation should include a UV stabilizer package validated by ASTM G154 or ISO 4892-2. Physical properties after 2,000 h of exposure should be compared against unexposed controls using tensile elongation retention per ASTM D638, with acceptance criteria agreed between the molder and the municipal end user. Products include two-wheeled refuse bins, park waste housings, and locking recycling carts.
Food processing plants adopt rotationally molded LLDPE fish tubs, brine chilling boxes, and meat lug liners because the material class withstands steam washing and quaternary ammonium sanitizer contact more effectively than many rigid amorphous materials, provided the part geometry does not contain sharp internal corners. For this service, wall thickness is normally 6 mm–12 mm, and the internal bottom-to-side radius should not be reduced below 25 mm; sharper radii act as stress concentrators under the swelling and cooling cycles of washdown. Sanitizer exposure is simulated by constant-strain immersion in a 2% quaternary ammonium chloride solution at 60°C for 7 days, followed by tensile property retention testing per ASTM D638. Direct food contact requires compliance with FDA 21 CFR 177.1520 for olefin polymers and, for the European market, EU 10/2011 overall migration limits. The compliance statement must also cover the green colorant in GRN 6229, the mold release agent, and any post-mold insulation materials; a raw resin food-contact letter alone is not sufficient for the finished double-wall tub. Insulated vessels are produced by molding an inner and outer shell separately and injecting a low-density two-part polyurethane foam between them. The foam free-rise density is typically 32–48 kg/m³, and the exotherm can exceed 120°C; the shell must be cooled below 50°C before foam injection to prevent distortion of the flat bottom surface. ESCR performance of the inner liner is assessed by ASTM D1693 in a nonylphenoxypoly(ethyleneoxy) ethanol solution at 50°C; the acceptance threshold should be set from the actual wall thickness and sanitizer concentration, not from a generic datasheet value. Published data for this specific colored grade in food contact service is limited, so validation should be performed on finished production samples. Products include insulated fish tubs, scallop boxes, and mobile meat lug dollies.
| Application segment | Governing standard or regulation | Measurement / property |
|---|---|---|
| Hazardous-liquid transport containers | UN Model Regulations design-type testing | Leakproofness, hydrostatic pressure, drop failure |
| Food contact fish tubs | FDA 21 CFR 177.1520, EU 10/2011 | Overall migration, extractable content |
| Outdoor weathering | ASTM G154, ISO 4892-2 | ΔE color shift, elongation retention |
| Environmental stress cracking | ASTM D1693, ASTM D5397 | Failure time in specified surfactant/notch condition |
| Rotomolding powder physical control | ASTM D1921, ASTM D1895 | Particle size distribution, bulk density |
Rotomolded municipal planter liners, park bollards, and playground tunnel sections consume green LLDPE powder where the precolored surface is a specification requirement rather than a post-mold paint replacement. These large, low-pressure parts are typically molded with wall thickness between 5 mm and 10 mm and are prone to parting-line thinning when the mold halves separate unevenly during heating. A parting-line gap as small as 0.2 mm can produce a visible flash line that must be trimmed and a thinner wall at the same location; mold clamps are therefore set to maintain closure pressure across the entire parting line. Molds with deep undercuts require a lower peak internal air temperature of 195°C–205°C to avoid sagging, while flat-section parts can use 210°C–220°C for maximum sintering. Zinc stearate or semi-permanent release agents are allowed for demolding, but excess release agent can migrate into the surface and reduce adhesion if post-mold polyurethane foam or silicone sealant is applied; release application should be kept below the minimum level needed for ejection. Full-scale outdoor weathering is validated by ASTM G154 or ISO 4892-2, and color shift is measured under CIE Lab conditions. These parts are not generally considered structural; they should not be used as fall-arrest or load-bearing components without a separate engineering review. Terminal products include municipal planter liners, park bench end panels, and playground tunnel tubes.
Competitive LyondellBasell Icorene 3545 GRN 6229 Polyethylene, Linear Low Density prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Rotational moulding of outdoor enclosures, agricultural water tanks and chemical storage vessels requires a polymer compound that can densify without shear, resist environmental stress cracking, and retain a stable pre-coloured surface after long oven residence. LyondellBasell Icorene 3545 GRN 6229 is a linear low-density polyethylene rotational moulding compound in which the Icorene 3545 base resin is pre-coloured green using manufacturer colour code 6229. The designation is conventionally read as indicating a nominal melt flow rate of 3.5 g/10 min when tested at 190°C under a 2.16 kg load in accordance with ISO 1133-1:2022 or ASTM D1238. The density class is near 0.945 g/cm³ according to ASTM D1505 or ISO 1183-1, placing it between conventional LDPE and HDPE. Because the 6229 green concentrate is compounded into the base resin, the melt flow rate, stabilizer package and density of the finished colour may differ slightly from unpigmented Icorene 3545; the lot certificate is the only reliable acceptance basis. Published data for this exact green configuration are limited; therefore, certified values from the supplier’s current technical datasheet should govern.
Compared with a high-pressure LDPE rotomoulding powder of similar melt flow rate, the Icorene 3545 GRN 6229 formulation provides higher tensile yield strength and higher resistance to environmental stress cracking because the linear backbone with short-chain branches resists craze propagation under external stress. Compared with a typical HDPE rotomoulding powder, the material exchanges some flexural stiffness and heat deflection capability for improved low-temperature impact and easier particle coalescence at lower peak internal air temperature. Compared with a metallocene LLDPE, the conventional Ziegler-Natta molecular architecture of this 3545 class may produce broader molecular weight distribution, faster bubble escape in thick sections, but lower ultimate dart impact at equivalent density and melt flow rate.
The numbers in the Icorene 3545 designation are commonly read as nominal melt-flow and density coordinates: approximately 3.5 g/10 min and 0.945 g/cm³. In rotational moulding, melt flow rate is not a direct viscosity value under process conditions, but it correlates inversely with zero-shear viscosity and directly with the rate at which molten polymer can flow into mould features such as threads, kiss-offs and reinforcing ribs. A compound with a melt flow rate below 2.0 g/10 min may require peak internal air temperatures above 215°C and longer oven residence to eliminate trapped gas; a compound with a melt flow rate above 6.0 g/10 min may sag in thick flat walls and produce unacceptable wall-thickness variation. The 3.5 g/10 min class is therefore a compromise for medium-to-large rotomoulded parts with nominal wall thickness in the 3–8 mm range.
The structural implications of the 3545 density class are also process-relevant. At approximately 0.945 g/cm³, the material is dense enough to develop adequate stiffness for self-supporting tanks, but not so dense that low-temperature impact falls into the brittle regime typical of high-density polyethylene. This distinction appears in comparative mechanical testing: the 3545 class commonly falls within 19–22 MPa tensile yield strength when tested according to ISO 527-2 at 23°C, while HDPE rotomoulding grades often exceed 24 MPa yield but may fracture at -40°C where the LLDPE remains ductile. The green 6229 pigment may act as a nucleating agent; therefore, the moulded part can show slightly higher crystallinity and shrinkage than natural powder, a difference that should be quantified before tooling dimensions are fixed.
Without twin-screw shear, rotational moulding densification proceeds through particle coalescence, bubble dissolution, and polymer melt densification. For this LLDPE class, the initial powder particle size distribution and dry-flow behaviour directly influence void content in the finished wall. A powder fraction retained on a 35-mesh sieve may require longer heat exposure than a finely ground powder; a high fraction of particles below 100 µm may improve surface smoothness but reduce dry-flow and increase the risk of agglomeration in humid plant air. The 6229 green compound should be stored indoors at low humidity, and powder temperature at charging should be above 15°C to reduce condensation.
Table 1 lists typical conditions used on carousel or shuttle machines for a 3545-class LLDPE green compound. These are not certified processing limits for every Icorene 3545 GRN 6229 application; they are starting points that must be confirmed with internal air temperature measurement.
| Parameter | Typical range | Measurement method |
|---|---|---|
| Oven setpoint | 285–315°C | shielded infrared pyrometer or oven thermocouple |
| Peak internal air temperature | 190–215°C | shielded thermocouple inside mould cavity |
| Mould rotation ratio | 3.5:1–4.5:1 | machine tachometer |
| Powder charge temperature | 15–35°C | contact thermocouple in powder bulk |
| Forced-air cooling until internal air falls below | 110°C | shielded thermocouple |
Peak internal air temperature is the controlling variable, not oven setpoint. Underheating to a peak internal air temperature below 180°C tends to leave spherical voids and grain boundaries in the inner wall; overheating above 220°C may consume antioxidant stabilizers prematurely and discolour thin sections. The green 6229 pigmentation can mask early oxidative yellowing, so surface gloss and tensile elongation loss are more reliable indicators of overbaking than colour change. Field measurements on shuttle machines with aluminium moulds of 6 mm nominal wall thickness indicate that a peak internal air temperature variation greater than ±8°C between cycles produces wall-thickness differences exceeding 0.5 mm in green LLDPE parts. The same variation occurs when powder charge temperature is allowed to fall below 15°C in a high-humidity plant; condensation on the powder increases apparent density and slows densification.
Across rotational moulding polyolefins, the property matrix is dominated by density and comonomer uniformity rather than melt flow rate alone. Table 2 presents class-level comparisons for the polymer families from which Icorene 3545 GRN 6229 is drawn. The values are representative of commercial rotomoulding compounds and should not replace lot-specific data for the pigmented grade.
| Attribute | Icorene 3545 GRN 6229 class | LDPE | HDPE | mLLDPE |
|---|---|---|---|---|
| Nominal density (g/cm³) | 0.940–0.950 | 0.920–0.930 | 0.945–0.965 | 0.930–0.940 |
| Melt flow rate at 190°C/2.16 kg (g/10 min) | 3.0–4.5 | 4.0–8.0 | 2.0–8.0 | 2.0–5.0 |
| Flexural modulus (MPa) | 900–1,200 | 350–700 | 1,200–1,600 | 600–900 |
| Environmental stress crack resistance rank | high | moderate | moderate-high | very high |
| Low-temperature impact rank | good | moderate | good | excellent |
| Surface smoothness after rotomoulding | moderate | high | moderate | high |
The practical difference between the 3545 class and a metallocene LLDPE appears in impact and processing latitude. Metallocene grades distribute comonomer more uniformly along the chain, which raises dart impact and ESCR but narrows the processing window; they may sag more readily when peak internal air temperature exceeds 210°C. The broad molecular weight distribution typical of conventional LLDPE yields a higher melt flow ratio and permits more rapid bubble dissolution in thick sections. This difference is not measured by melt flow rate alone, so incoming quality checks should include melt flow ratio, apparent density, and dry-flow tests such as those referenced in ASTM D1895.
For outdoor service, the green 6229 pre-colour provides opacity and ultraviolet screening, but it is not a substitute for a hindered amine light stabilizer and antioxidant package. The supplier-approved weathering package should be verified under accelerated ageing according to ASTM G154 or ISO 4892-2, and outdoor performance should be correlated with Florida or Arizona exposure data if available. Published test data for this exact green code are limited; therefore, a purchaser should obtain weathering retention data from the current LyondellBasell technical datasheet before specifying the compound for a 5-year or 10-year outdoor service interval.
Environmental stress crack resistance is relevant for tanks and containers exposed to surfactants, agricultural chemicals, or sodium hypochlorite. The 3545 class LLDPE generally provides higher ESCR than LDPE and HDPE when tested under ASTM D1693-15 in a representative stress cracking agent. However, ESCR is sensitive to colourant dispersion; poorly dispersed green masterbatch particles can act as stress risers. Incoming inspection should therefore include sieve analysis of the powder and a melt-filtered dispersion check, not solely density and melt flow rate.
From a chemical compatibility standpoint, Icorene 3545 GRN 6229 should not be used with strong oxidizing acids, chlorinated solvents, aromatic hydrocarbons, or concentrated sodium hypochlorite above 5% at elevated temperature without immersion testing according to ASTM D543. Contact with oxidizing agents at 60°C can reduce elongation at break long before visible degradation appears. Food-contact suitability should not be assumed; compliance with FDA 21 CFR 177.1520 or EU Regulation 10/2011 must be confirmed in writing for the specific green concentrate, because pigment packages are frequently outside the scope of unpigmented food-contact clearances.
The grade is best reserved for medium-to-large rotomoulded parts such as agricultural tanks, outdoor enclosures, and general industrial containers where a pre-coloured green surface, balanced stiffness, impact resistance and ESCR are required. Processors using regrind should limit ground fallback to 10–20% by weight, because higher regrind content increases the proportion of heat-damaged resin, reduces dry-flow and can shift peak internal air temperature demand upward. Before producing water-contact or chemical-contact parts, validation of the complete end-use article under the relevant national standards is required.
Because Icorene 3545 GRN 6229 is a pre-coloured compound, incoming inspection based solely on density and melt flow rate can miss changes in pigment dispersion, powder dry-flow, and heat history. A rotomoulding-specific quality plan should include apparent density and dry-flow according to ASTM D1895, sieve analysis of the powder, melt flow rate according to ISO 1133-1:2022, density according to ASTM D1505, and moisture content by loss-on-drying or Karl Fischer. Moisture content above 0.05 wt% can generate steam during the oven cycle and produce voids or surface pinholes. Powder received in cold weather should be conditioned to 15–35°C before charging.
Lot-to-lot variation in the 6229 green concentrate may shift crystallisation onset temperature. A practical control is to prepare a moulded test plaque from each incoming lot on a laboratory rotational moulding cell and compare peak internal air temperature, shrinkage, and Gardner impact according to ASTM D5420 or falling dart impact according to ISO 6603-2 against the previously approved lot. A shift in shrinkage of more than 0.2% indicates that tooling dimensions may need adjustment or that the pigment nucleating effect has changed.
Batch-to-batch variation can appear as brittleness in colder environments. Low-temperature impact evaluation should be conducted at the minimum service temperature, frequently -20°C or -40°C, not only at 23°C. The test type should match the failure mode: uniaxial tensile impact may not capture the biaxial stress state of a rotomoulded tank wall. A falling dart method such as ASTM D5628-18 or ISO 6603-2 is closer to field impact.
The 3545 GRN 6229 product is not recommended for high-temperature industrial service above 80°C continuous unless the specific application is validated under ASTM D2990 creep and ASTM D638 tensile retention. Above this temperature, oxidative stabilizer consumption accelerates, and dimensional stability under load decreases. For intermittent exposure to hot water, the user should test the complete part under the relevant service pressure and thermal cycle, because moulded-in stresses from thick-to-thin transitions can dominate long-term failure.