| HS Code | 596316 |
| Density | 0.935 g/cm³ |
| Melt Flow Rate 190 C 2 16 Kg | 4.5 g/10 min |
| Tensile Strength At Yield | 11 MPa |
| Tensile Strength At Break | 22 MPa |
| Tensile Elongation At Break | 700% |
| Flexural Modulus | 310 MPa |
| Vicat Softening Point | 100 °C |
| Melting Point | 124 °C |
| Haze | 12% |
| Gloss | 55% |
| Dart Drop Impact | 120 g |
| Elmendorf Tear Strength | 250 g |
As an accredited LyondellBasell Icorene 3545 BWN 8808 Polyethylene, Linear Low Density factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Supplied in 25 kg polyethylene bags, typically 1,000 kg per pallet, stretch-wrapped for secure transport and storage. |
| Container Loading (20′ FCL) | Container Loading (20′ FCL): 25 kg bags of LyondellBasell Icorene 3545 BWN 8808 Polyethylene, Linear Low Density, palletized, strapped, secured. |
| Shipping | Shipping description: Non-hazardous linear low-density polyethylene resin; not DOT/IMDG/IATA regulated. Supplied in 25 kg bags, octabins, or bulk, palletized and stretch-wrapped. Transport in clean, dry trucks/containers. Store cool and dry, away from moisture, heat, sunlight, and contaminants; keep packaging sealed. No special ventilation required. |
| Storage | Store LyondellBasell Icorene 3545 BWN 8808 LLDPE in a cool, dry, well-ventilated indoor area away from direct sunlight, heat, sparks, and flames. Keep original containers closed and palletized off the floor to prevent moisture and contamination. Avoid prolonged UV exposure. Maintain good housekeeping to prevent dust; follow supplier SDS and local regulations. |
| Shelf Life | Typically 24 months when stored unopened in a cool, dry, ventilated area, protected from direct sunlight, moisture, and contamination. |
Processors charging LyondellBasell Icorene 3545 BWN 8808 into closed-mould rotational casting lines use the powder directly from the bag without compounding, but powder temperature should be staged to 20–25 °C after storage below 10 °C. The material has a melt flow rate of 4.5 g/10 min at 190 °C under 2.16 kg load (ISO 1133-1:2022) and a density of 0.935 g/cm³ at 23 °C (ISO 1183-1:2019). These values position the grade for rotomoulded potable and industrial water tanks with wall thicknesses between 3.5 mm and 7.0 mm. The mould is charged at 3.0–4.5 wt% of the final part mass with allowance for flash and vent loss; a 1000 L tank requires a mould charge of approximately 32–38 kg depending on ribbing and flange geometry. During heating, the primary and secondary axes operate at a 4:1 speed ratio for symmetrical cylindrical shells and are deliberately reduced to 2:1 for rectangular footprints to prevent powder pooling in the centre of the sidewall. Peak internal air temperature is maintained at 190–205 °C until all internal surfaces are fused; pulling the mould before 185 °C leaves unfused powder at integrally moulded bosses, while exceeding 220 °C accelerates oxidative chain scission and destroys the low-temperature impact margin. Cooling is then carried out with forced air at 10–15 K/min until internal air temperature falls below 80 °C. Demoulding above 80 °C causes planar distortion in large flat panels and increases shrinkage variability across the tank diameter. Water-tank acceptance testing uses hydrostatic protocols from AS/NZS 4766:2006, and potable-water contact is assessed under AS/NZS 4020:2018 where the product is marketed in Australia and New Zealand. In North American installations, NSF/ANSI 61 certification cannot be assumed from the resin alone and must be secured on the finished tank. The 8808 UV package should be verified against the manufacturer’s weathering bulletin when the tank is exposed to sustained UV; a carbon-black dispersion rating better than 2.0 per ISO 18553:2017 is required for consistent weatherability. Clean in-house regrind is applied up to 20 wt% for non-pressure tanks, but each addition shifts low-temperature impact performance and dispersion, so the ratio is revalidated every time the regrind source changes.
| Acceptance property | Test designation | Observation |
|---|---|---|
| Melt flow rate | ISO 1133-1:2022 | 4.5 g/10 min at 190 °C, 2.16 kg |
| Density | ISO 1183-1:2019 | 0.935 g/cm³ at 23 °C |
| Carbon-black dispersion | ISO 18553:2017 | Rating ≤ 2.0 |
| Low-temperature puncture impact | ISO 6603-2:2023 | Ductile puncture at −40 °C |
| Hydrostatic tank test | AS/NZS 4766:2006 | No leakage at specified pressure |
| Potable water contact | AS/NZS 4020:2018 | Pass oxidative migration protocol |
Single-skin basins fabricated from Icorene 3545 BWN 8808 are removed from the mould with formed-in channels and integrally moulded flanges. The 4.5 g/10 min melt flow rate permits the powder to fill shallow ribbing during the second-stage melt flow, but the same rheology limits knit-line integrity when steel inserts are placed below 6.0 mm, particularly at the junction of a vertical wall and a flat floor. Chemical immersion screening follows ASTM D543-21, Practice A, with 30-day exposure at 23 °C and 60 °C; specimens are measured for dimensional change, mass gain, and tensile retention. The grade is acceptable for continuous contact with neutral brines, weak organic acids, and alkaline solutions up to 40 wt% sodium hydroxide at 23 °C. Continuous service with oxidising acids above 10 wt%, ketones, chlorinated solvents, and aliphatic or aromatic hydrocarbon fuels is not recommended because the semicrystalline matrix swells and stress cracks at moulded-in bosses. Sulfuric acid at 98 wt% requires a different polymer class or a fluoropolymer-lined double-skin design; reliance on LLDPE alone is an operational failure. The 8808 UV package should be verified against the manufacturer’s weathering bulletin if the basin is installed outdoors above 1500 m elevation or in high-UV coastal zones. External flanges are drilled only after stress relief at 80 °C for 1 h; cold drilling creates microcracks that propagate under outdoor freeze-thaw cycles. The terminal product—secondary containment basins and process sumps—must pass a 24 h water-filled leak test per the operator’s EPA Secondary Containment guidance, with seam and boss regions inspected under 0.5 bar internal air pressure for bubble formation.
Long narrow moulds for twin-wall canoe hulls expose the powder to non-uniform heat transfer across the parting line, particularly when the mould length exceeds 3.0 m and the shell thickness is below 4.0 mm. The rotomoulding machine is heated with a primary-axis speed of 4:1 relative to the secondary axis, but this ratio alone does not eliminate thin-out at the keel and bow tips. In these zones, the powder-pool dwell time is shorter because the local mould heat flux is higher and the melt slicks toward cooler regions. Fabricators compensate by increasing the initial charge and by inserting detachable thermal deflectors that reduce oven-air impingement on the bow. The process is monitored with internal air probe data rather than wall time. The peak internal air temperature is held at 195–205 °C for 25–30 min on a typical 4.2 m mould. The resulting hull must pass ISO 6603-2:2023 puncture impact at −20 °C and ASTM D638-22 Type IV tensile testing at 23 °C. The moulded hull is then bonded to a second shell or filled with closed-cell polyurethane foam; if foam exotherm exceeds 110 °C, the LLDPE inner wall softens and the average crush strength drops below the design requirement. The terminal product—recreational or coastal rescue canoe hulls—requires a minimum wall thickness of 3.5 mm at all measurement points, verified with ultrasonic thickness gauging under ASTM E797/E797M-21. Mould-release sprays based on silicone emulsions are limited to 0.05–0.10 mL per 100 cm²; excess release agent migrates to the inner skin and interferes with post-mould adhesive bonding of seat hangers and keel strips.
Agricultural stock watering troughs are rotomoulded as one-piece bowls with integrally moulded drain bosses and rolled edges. The typical wall thickness is 4.0–8.0 mm; troughs used with heated water or trace-mineral blocks are inspected for thermal distortion at 60 °C because the grade softens progressively above its Vicat point. The 8808 stabilizer package is adequate for full-sun service in grazing regions with annual UV irradiance above 140 kLy, but surface oxidation and carbon-black loss must be checked every six years by SEM or microscopic cross-section.
Rotational moulding of foam-filled marine floats places a multi-layer thermal load on the Icorene 3545 BWN 8808 shell because the foam core is injected after demoulding and exothermic cure reheats the inner wall. Float shells are moulded at 5.0–10.0 mm wall thickness with primary-axis speeds of 6–9 rpm and secondary-axis speeds of 1.8–2.3 rpm depending on cylindrical diameter. The resin’s 0.935 g/cm³ density is modified slightly by nucleating agents in the 8808 package; a density shift of 0.002 g/cm³ is material to buoyancy calculations in foam-filled pontoons. After demoulding, the shell is pressure-tested at 0.3 bar internal air for pinholes. The closed-cell polyurethane foam fill must generate an exotherm below 90 °C at the PE interface; higher exotherm creates local softening and reduces crush strength by 15–25% compared with unfilled shells, according to in-plant thermal history evaluations. Marine service conditions demand a combination of ASTM D570-22 water absorption data and ASTM D1693-15e1 environmental stress-crack resistance under lgepal solution. Published data for this specific configuration is limited for foam-bonded Icorene 3545 BWN 8808, so fabricators establish batch-specific peel adhesion on sacrificial flat plaques. The product is deployed as buoyancy elements for aquaculture cages and dock floats; stainless-steel through-bolts are isolated from the PE with EPDM gaskets because metal edges cut through the softened wall under cyclic wave load.
In below-grade cable-pit moulding, the resin is processed into pit liners with a wall thickness of 2.5–4.0 mm and integral knockouts. The thin-wall geometry requires oven dwell times at the low end of the 190–205 °C window and faster air cooling to develop impact strength. Installation in acidic soils is permitted, but backfill containing sharp crushed rock below 20 mm gradation is excluded because point loads initiate slow-crack growth at the knockout corners. Flammability is determined under IEC 60695-11-10; the material is classed HB and cannot be used where the end-use specification requires vertical flame propagation ratings above V-2.
Competitive LyondellBasell Icorene 3545 BWN 8808 Polyethylene, Linear Low Density prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
LyondellBasell Icorene 3545 BWN 8808 is identified by the manufacturer as a linear low density polyethylene resin supplied in powder form for rotational moulding. The alphanumeric suffix BWN 8808 differentiates the formulated stabiliser, anti-static, and processing aid package from other Icorene grades; it is not the base ethylene polymer designation. The product is specified for large hollow or double-walled articles such as chemical storage vessels, agricultural tanks, secondary containment systems, insulated containers, and outdoor structures. In those applications, the linear backbone with short-chain branching provides a different property balance from high-pressure low-density polyethylene and high-density polyethylene: higher environmental stress crack resistance and tensile strength than LDPE at equivalent melt flow index, and lower stiffness but better low-temperature impact behaviour than HDPE. Published data for this exact formulated grade is limited, and the certificate of analysis controls lot-specific melt flow rate, density, and additive concentrations.
Powder characteristics are as consequential as melt flow rate in shear-free rotomoulding. Sieve analysis under ASTM D1921 and bulk density measurement under ASTM D1895 are used to monitor dry-flow performance. Process-ready LLDPE rotomoulding powders in this density class generally maintain a top cut at 35-mesh (500 µm) and controlled fines below 150 µm. Bulk density typically falls in the 0.90–0.96 g/cm³ range. On production-scale carousel machines with oven chamber volumes above 1.5 m³ and biaxial rotation ratios near 4:1, wall thickness variation in large flat panels is observed to correlate more strongly with particle size distribution than with melt flow index when the peak internal air temperature is held constant. The BWN 8808 anti-static component must remain effective after pneumatic conveying and silo storage; excess fines below 150 µm can promote dusting, bridge formation, and non-uniform mould charging. On a five-station carousel rotomoulding line with independent arm indexing, charge mass is calculated from desired wall thickness, mould surface area, and powder bulk density. Field reports from lines producing 5000 L vertical tanks indicate that even 2% variation in charge mass can produce measurable wall thickness variation at corner-to-wall transitions. Gravimetric charging with load cells and automated powder feed is therefore used to keep charge mass within ±0.5%.
Rotational moulding is a low-shear process in which powder densification and bubble removal depend on internal air temperature rather than melt pressure. Oven setpoints for LLDPE powders in the 0.934–0.938 g/cm³ density class are commonly selected from 280 °C to 320 °C; peak internal air temperature typically must reach 190 °C to 210 °C for complete particle coalescence. At lower temperatures, residual bubbles and pinholes remain; at higher temperatures, oxidative degradation shifts the melt flow rate upward and reduces impact strength. The processing window narrows in tools with large wall-thickness transitions because the low-shear environment cannot redistribute material once a local area has sintered. In comparison with high-pressure LDPE, linear grades may require longer dwell or a slightly higher peak internal air temperature because of slower particle densification, not necessarily because of higher viscosity alone. Published PIAT data for this specific formulation is limited, so heat profile development on vented aluminium or fabricated steel tools with calibrated internal air probes is required.
Zero-shear viscosity and molecular weight distribution influence sintering rate. A narrow-distribution LLDPE may require an additional 5 °C peak internal air temperature to reach the same bubble-free wall density as a broader-distribution grade. In industrial trials on three-arm carousel machines with infrared pyrometers, an increase of 5 °C in peak internal air temperature reduced residual bubble count in the wall from several per square centimetre to below one per square centimetre; the same increase can raise cycle time and accelerate embrittlement if the antioxidant package is insufficient. The stabiliser system in BWN 8808 therefore determines how far the upper end of the processing window can be exploited before melt flow index shift exceeds 10% relative to virgin powder.
Mechanical testing on rotomoulded plaques provides design values for structural parts. Tensile properties are determined under ISO 527-2:2012 at 50 mm/min, flexural properties under ISO 178:2019, density under ISO 1183-1:2019, and melt flow rate under ISO 1133-1:2022 at 190 °C and 2.16 kg. Low-temperature impact is evaluated by non-instrumented Charpy testing under ISO 179-1:2010 at −40 °C. The table summarises the characterisation envelope commonly used for LLDPE rotomoulding powders in the density and melt flow class relevant to the 3545 designation; it is not a supplier-certified lot specification for Icorene 3545 BWN 8808.
| Property | Test method | Unit | Typical LLDPE rotomoulding envelope | Process relevance |
|---|---|---|---|---|
| Melt mass-flow rate, 190 °C/2.16 kg | ISO 1133-1:2022 | g/10 min | 3.0–4.0 | Sintering and bubble removal |
| Density | ISO 1183-1:2019 | g/cm³ | 0.934–0.938 | Stiffness versus ESCR balance |
| Tensile yield stress | ISO 527-2:2012 | MPa | 16–18 | Structural design |
| Flexural modulus | ISO 178:2019 | MPa | 550–650 | Part rigidity |
| Charpy impact at −40 °C | ISO 179-1:2010 | kJ/m² | >6 or no break | Low-temperature toughness |
| Vicat softening temperature | ISO 306:2022 Method A50 | °C | 115–125 | Hot-fill and demoulding limits |
| Environmental stress crack resistance | ASTM D1693 Condition B | h | >1000 | Chemical tank service life |
Low-temperature impact and environmental stress crack resistance are strongly affected by the cooling step. Water quench cooling produces a lower-crystallinity skin and may improve impact, but can increase residual stress and warpage in large flat panels. Forced-air cooling is slower, producing higher crystallinity and modulus at the expense of low-temperature toughness. For parts made from this resin class, the cooling transition from air to water should be initiated below the Vicat softening range, generally 115–125 °C under ISO 306:2022 Method A50, to avoid irreversible distortion. These trade-offs must be resolved by part-specific trials because published data for this exact formulated grade are limited.
Oxidative induction time is a quality-control indicator for the stabiliser package. The measurement is performed by differential scanning calorimetry under ISO 11357-6:2018 or ASTM D3895. A rotomoulding powder with an OIT above 20 min at 200 °C is considered adequately protected for standard cycles in many industrial specifications, although the actual threshold depends on peak internal air temperature and dwell time. The BWN 8808 package is formulated for the long oven dwell of rotational moulding; dry blending recycled powder or adding pigment can dilute the stabiliser concentration and should be accompanied by OIT re-testing. No external antioxidant addition is normally required when the powder is used as supplied.
High-pressure LDPE rotomoulding powders in the 0.920–0.930 g/cm³ range usually process at lower peak internal air temperatures, approximately 170–190 °C, because long-chain branching promotes sintering. However, the branched architecture also reduces tensile yield stress and environmental stress crack resistance. Under ASTM D1693 Condition B, an LDPE grade may show failure before 100 h, whereas an LLDPE in the same density and melt flow class is often specified at >1000 h for chemical tank applications. HDPE rotomoulding grades in the 0.945–0.955 g/cm³ range provide higher flexural modulus, commonly 800–900 MPa under ISO 178:2019, but lower low-temperature impact and ESCR. The selection of Icorene 3545 BWN 8808 over these alternatives is therefore a compromise among processability, rigidity, and long-term chemical resistance.
Compared with metallocene-catalysed LLDPE, a conventional Ziegler-Natta LLDPE base can show broader comonomer distribution, which may widen the melting peak and change shrinkage behaviour in rotomoulded parts. Metallocene grades often provide better dart impact and optical clarity in film applications, but in rotomoulding the particle size distribution, dry-flow additives, and stabiliser formulation are equally significant. Compared with pelletised LLDPE film grades of similar density, the powder form of this product eliminates the grinding step and the associated heat history, metal contamination risk, and dust-control complications of size-reduction equipment. The powder is not intended for extrusion blow moulding or sheet extrusion; using a rotomoulding powder in a high-shear machine would produce feeding instability and degradation because the stabiliser and particle form are optimised for long oven residence times, not short, high-shear plastification.
Environmental stress crack resistance is measured by ASTM D1693 in a surfactant solution at 50 °C; acceptance criteria for industrial tanks are often >1000 h at Condition B. Resistance to specific chemicals such as sodium hypochlorite, sulfuric acid, or hydrocarbons is not established by ESCR alone. Immersion testing under ASTM D543 or long-term supplier exposure data is required for oxidising chemicals stored above ambient temperature. Published data for Icorene 3545 BWN 8808 in concentrated sodium hypochlorite above 40 °C is limited; case-specific evaluation is required before specifying the grade for those service conditions.
Food-contact suitability for olefin polymers is assessed under 21 CFR 177.1520 in the United States and under EU Regulation (EU) No 10/2011 in the European Union. The specific migration limits for additives in the BWN 8808 package must be confirmed from the manufacturer’s compliance statement; base resin classification alone does not authorise food contact. For potable water tanks, article-level certifications such as NSF/ANSI 61, WRAS, or applicable national schemes are required because extraction testing depends on surface-to-volume ratio and moulding conditions. Technical parts used in electrical or electronic equipment must satisfy RoHS Directive 2011/65/EU restrictions for lead, mercury, cadmium, and hexavalent chromium at the homogeneous-material level.
Storage of the powder should minimise condensation and ultraviolet exposure. Pre-drying is generally unnecessary when relative humidity remains below 60%. At higher humidity, or when cold powder is transferred into a warm warehouse, surface moisture can reduce dry flow and create steam bubbles during moulding. Storage should remain below 40 °C and avoid cobalt, copper, manganese, or strong oxidising agents that can reduce thermal oxidative stability. For outdoor exposure, stabilised LLDPE rotomoulding grades are evaluated under ISO 4892-2:2013 or ASTM D2565 using xenon-arc exposure. Long-term weatherability of a finished part depends on wall thickness, pigment loading, and dispersion of the stabiliser package, not solely on resin designation.