| HS Code | 133452 |
| Density | 0.935 g/cm³ |
| Melt Flow Rate 190 C 2 16 Kg | 3.5 g/10 min |
| Tensile Strength At Yield | 13 MPa |
| Tensile Strength At Break | 22 MPa |
| Elongation At Break | 800% |
| Flexural Modulus | 550 MPa |
| Shore D Hardness | 50 |
| Vicat Softening Temperature | 100 °C |
| Melting Temperature | 123 °C |
| Deflection Temperature At 0 46 Mpa | 70 °C |
| Deflection Temperature At 1 8 Mpa | 50 °C |
| Thermal Conductivity | 0.33 W/m·K |
As an accredited LyondellBasell Icorene 3545 BUE 5524 Polyethylene, Linear Low Density factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | LyondellBasell Icorene 3545 BUE 5524 Linear Low Density Polyethylene comes in 25 kg bags, palletized and stretch-wrapped. |
| Container Loading (20′ FCL) | Container Loading (20′ FCL): LyondellBasell Icorene 3545 BUE 5524 Linear Low Density Polyethylene, securely palletized and stowed for ocean shipment. |
| Shipping | LyondellBasell Icorene 3545 BUE 5524 Polyethylene, Linear Low Density is a non-hazardous polymer pellet. It is typically shipped in 25-kg bags or bulk containers, palletized and wrapped. Not classified as dangerous goods for DOT, IMDG, IATA, or ADR. Keep dry, clean, and away from heat and direct sunlight. |
| Storage | Store in a cool, dry, well-ventilated area away from direct sunlight, heat, sparks, flames, and strong oxidizers. Keep containers tightly closed and palletized to prevent moisture, dust, and contamination. Avoid prolonged UV exposure and temperatures above 50°C. Maintain good housekeeping; spilled pellets can create slippery surfaces. Use original packaging and follow local regulations. |
| Shelf Life | Typically 24 months when stored in original, unopened packaging under cool, dry conditions, away from direct sunlight and moisture. |
LyondellBasell Icorene 3545 BUE 5524 enters downstream processing as an LLDPE rotomoulding powder produced by grinding pellet feedstock to a nominal 35 mesh particle size distribution; the as-supplied datasheet lists density at 0.935 g/cm³ and melt flow index at 5.5 g/10 min under 190°C/2.16 kg when tested to ISO 1133-1:2022. In rotomoulded closed-head chemical storage tanks and intermediate bulk container outer shells, the powder is dry-charged into steel or aluminium moulds at 0.38–0.42 g/cm³ apparent density, with sieve retention above 600 µm held below 5% because coarse fractions create unmelted inclusions at wall thicknesses below 4 mm. The oven is set at 280–310°C and the peak internal air temperature is held at 185–195°C for 8–12 min; premature demoulding before the inner surface cools to 120°C produces sidewall warpage on flat vertical panels. For a 1,000 L tank with 5 mm nominal wall, charge weight is maintained at ±0.5 wt% to prevent excess polymer accumulation at the pole opposite the rotational axis. Parting-line fusion is checked by destructive sectioning at the mould flange; cold-fusion lips appear when the biaxial rotation ratio drifts below 3:1, which is a recurring production failure mode on shuttle-type rotational moulding machines. Chemical resistance is restricted to intermittent contact with dilute aqueous acids, alkalis and non-oxidising salt solutions up to 40°C; continuous exposure to aromatic hydrocarbons, chlorinated solvents or strong oxidising acids at ambient temperature promotes environmental stress cracking. Powder conditioning at 40°C for 4 h is required when storage relative humidity exceeds 60%, otherwise surface moisture generates steam pinholes in the outer skin. Potable-water and food-contact tanks require verification against FDA 21 CFR §177.1520 and EU Regulation (EU) No 10/2011, with overall migration below 10 mg/dm² under the intended food simulant.
Above-ground irrigation and rainwater reservoirs from 2,000 L to 5,000 L operate under daily drawdown and refill, which places the sidewall ribs under cyclic hoop strain of 0.5–0.8%. The critical design property is environmental stress-crack resistance measured by ASTM D1693-15 condition B in 10% Igepal CO-630 at 50°C; rotomoulded LLDPE parts typically fail after 1,000 h when the inner wall is not fused above 190°C. Slow cooling through 115°C to 85°C is necessary to minimise residual shrinkage stress, because water quenching from 190°C to 70°C freezes in micro-crazes that propagate after the first season of fertiliser contact. Agrochemical storage acceptance tests use 10 wt% urea and 5 wt% ammonium sulphate solutions at 40°C for 30 days, followed by tensile elongation testing to ISO 527-2:2012; retained elongation above 600% indicates acceptable chemical resistance for dilute agricultural liquids. Outdoor weathering of the pigmented outer layer is benchmarked by ISO 4892-2:2013 cycle 1 for 5,000 h, after which the carbon black-containing compound should retain at least 80% of the original elongation at break. Moulders running unpigmented or lightly tinted parts should not reduce oven temperature below 280°C to compensate for colour shift, because incomplete fusion of the inner surface causes pinholes at the tank bottom radius. Rotation speed on the major axis is held at 7–9 rpm, with a minor axis setting of 2–3 rpm, to avoid powder tunnelling inside the mould and to maintain uniform wall thickness at the drain boss and baffle joints. When liquid fertiliser contact is continuous rather than intermittent, a dedicated chemical liner or a higher-density polyethylene grade should be selected, because LLDPE stress-cracking resistance decreases with increasing polar liquid sorption at temperatures above 35°C.
For double-wall dock floats and aquaculture cage collars, the mould is charged with natural or black-pigmented powder and rotated with a filling port that permits insertion of a closed-cell polyurethane foam core after the LLDPE shell has cooled to 40°C or lower. The outer wall is typically 5–8 mm thick and the mould contains aluminium lifting lugs positioned as heat sinks during oven dwell. The oven is operated at 300–320°C to compensate for the thermal mass of the metal insert, and the peak internal air temperature is extended to 195–205°C for 12–15 min. A production failure mode occurs when the aluminium insert exceeds 80°C during the polyurethane exotherm, producing local core collapse adjacent to the lug; thermally breaking the insert with a polymer bush reduces the interfacial temperature by 15–20°C. The inner LLDPE surface is mechanically roughened to 50–80 µm Ra before foam filling to provide mechanical keying, because the untreated surface energy of polyethylene is below 32 mN/m and adhesive bonding to polyurethane is otherwise limited. Water absorption of the moulded shell is below 0.01% after 24 h immersion per ASTM D570, and low-temperature dart impact at -20°C using a 5 kg striker from 1.0 m shows no brittle puncture on foam-filled panels. For marine service, the outer surface should be compounded with 2–2.5 wt% carbon black or an equivalent UV-stabiliser package, and the finished part is inspected by ultrasonic thickness mapping at the radii and weld line; thickness deviation greater than ±15% from nominal is rejected due to the risk of buckling under wave loading. Service in continuous sunlight with salt spray requires a 3,000 h xenon arc test per ISO 4892-2:2013 and a salt-spray exposure per ISO 9227:2022 for 1,000 h, after which the tensile elongation should remain above 500%. Published data for this specific marine configuration with Icorene 3545 BUE 5524 is limited; the above thresholds are derived from standard LLDPE rotomoulding practice and should be confirmed through part-level qualification.
In freezer-rated food handling boxes and insulated bin shells rated for -30°C service, wall thickness is maintained between 6 mm and 8 mm and the minimum corner radius is held at 12 mm to prevent notch-like stress concentration at the base junction. Moulders set the oven at 290–300°C and use a 4:1 rotation ratio, with the major axis at 8 rpm and the minor axis at 2 rpm, to maintain thickness uniformity at the rim and base. Air cooling is continued to 80°C before demoulding; release at higher core temperature causes the long sidewalls to bow inward and creates a visible flatness defect. Cold impact is assessed at -30°C with a 5 kg steel dart dropped from 1.0 m onto the inner base, with acceptance limited to no crack longer than 5 mm. Fatty food contact requires migration testing in 95% ethanol or isooctane at 40°C for 10 days under EU Regulation 10/2011, and the overall migration limit is 10 mg/dm². Polyurethane foam insulation is injected after shell moulding; the foam cavity must be dry and free of release-agent residues, because silicone-based mould release reduces foam adhesion and causes voids detectable by thermal imaging after a 24 h conditioning cycle at 23°C.
| Application | Typical wall thickness | Oven temperature | Peak internal air temperature | Critical control |
|---|---|---|---|---|
| Chemical storage tanks | 4–6 mm | 280–310°C | 185–195°C | Parting-line fusion, moisture content |
| Agricultural reservoirs | 5–8 mm | 280–310°C | 190–200°C | ESCR, slow cooling through 115°C |
| Marine float shells | 5–8 mm | 300–320°C | 195–205°C | Insert heat sink, PU foam exotherm |
| Freezer food boxes | 6–8 mm | 290–300°C | 190–200°C | Corner radius, migration compliance |
Outdoor playground slides, tunnel sections and climbing panels are rotomoulded in double-wall configurations with a nominal outer shell thickness of 5 mm and an outer layer compounded with a hindered amine light stabiliser package. Procurement specifications commonly require 5,000 h accelerated weathering under ISO 4892-2:2013 method A, cycle 1, followed by a tensile test at 23°C per ISO 527-2:2012; the retained elongation at break should exceed 400%. Surface cracking that appears before 3,000 h is a failure signal indicating either insufficient UV stabiliser or excessive wall oxidation caused by oven dwell above 300°C. In production trials with orange and yellow moulded panels, colour shift ΔE greater than 3.0 after 2,000 h is observed when the same base compound is processed with a peak internal air temperature above 200°C; this indicates that oven-induced degradation consumes the stabiliser package before the service exposure begins. Structural safety of the installed component is assessed under EN 1176-1:2017 for playground equipment, with entrapment openings checked against the 8 mm hinge and head probe dimensions, while impact attenuation of the surrounding surface is verified by EN 1177:2018 using the head injury criterion method. Moulders are advised to maintain rotation ratio at 4:1 and to purge the mould cavity with dry air when ambient relative humidity exceeds 60%, because trapped moisture on the powder surface produces surface blisters that become crack initiation sites after outdoor freeze-thaw cycling.
Vehicle-mounted wash-water tanks and cab interior liner modules produced from Icorene 3545 BUE 5524 are rotomoulded with aluminium tools and internal baffles that act as heat sinks, requiring a charge mass factor of 0.9–1.1 times the theoretical part weight. Insufficient charging on production lines creates thin spots below 3 mm at the baffle radius, and ultrasonic thickness mapping shows negative deviation of 20–30% from the nominal wall. Interior liner specifications include odour and fogging evaluation according to VDA 278:2018 and ISO 6452:2021; the grade is normally used in compounded form with a low-fogging stabiliser package, but the condensation value limit is defined by the individual OEM specification, and published data for this specific automotive configuration is limited. Tensile yield stress is measured in the range 14–16 MPa and flexural modulus in the range 500–600 MPa per ISO 527-2 and ISO 178:2019, supporting brass insert attachment bosses up to M8 when the edge distance is at least 14 mm and the boss diameter is at least 2.0 times the insert outside diameter. Underhood and cab interior parts should be validated for continuous service above 60°C only with heat-aging tests per ISO 188:2011 at 100°C for 168 h; this LLDPE grade is not recommended for direct fuel contact or for components that require sustained creep resistance above 70°C.
| Regulation or standard | Scope | Threshold or method |
|---|---|---|
| FDA 21 CFR §177.1520 | Olefin polymers for food contact | End-test compliance for intended food simulant |
| EU Regulation (EU) No 10/2011 | Plastic materials in food contact | Overall migration 10 mg/dm² |
| RoHS Directive 2011/65/EU, Annex II | Electrical and electronic equipment | Lead 0.1 wt%, cadmium 0.01 wt% in homogeneous material |
| REACH Regulation (EC) No 1907/2006, Article 33 | Substances of very high concern | Notification if SVHC > 0.1% w/w in article |
| EN 1176-1:2017 and EN 1177:2018 | Playground equipment and surfacing | Entrapment and impact attenuation criteria |
Competitive LyondellBasell Icorene 3545 BUE 5524 Polyethylene, Linear Low Density prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
LyondellBasell Icorene 3545 BUE 5524, a linear low-density polyethylene grade for rotational moulding, is supplied as a powder and specified primarily through its nominal density of 0.935 g/cm³ and melt flow rate of 4.5 g/10 min under 190 °C/2.16 kg loading in ISO 1133-1:2022. The 3545 designation reflects the density-melt-flow pairing; the BUE suffix is associated with butene comonomer incorporation, and the 5524 extension identifies an ultraviolet stabilization package. These compositional features place the resin in the intermediate crystallinity range between low-density polyethylene and medium-density polyethylene; the lower density reduces flexural stiffness but expands the amorphous tie-chain population that governs low-temperature ductility. The grade is used in rotationally moulded outdoor articles such as water tanks, agricultural hoppers, furniture, and recreational components, where a combination of moderate rigidity, sub-zero impact resistance, and UV stability is required.
The butene-derived short-chain branching in Icorene 3545 BUE 5524 interrupts lamellar crystallization but does not produce the same long-chain intermolecular entanglement as an octene comonomer at equivalent density. This molecular difference is significant for rotomoulded parts under sustained hydrostatic or detergent-related stress. Environmental stress crack resistance measured under ASTM D1693 Condition B in 10% Igepal CO-630 at 50 °C is typically reported above 1000 h for this grade, but this value is lower than that of many octene-based LLDPE rotomoulding powders of identical melt flow rate. The butene architecture also reduces dart impact and puncture propagation at sub-zero temperatures. In practice, the material is selected where stress crack severity is moderate; for continuous immersion in aggressive surfactants or high-solvent agricultural chemicals, an octene-based LLDPE or a cross-linked high-density polyethylene would provide a higher ESCR safety margin.
For injection moulding and compounding comparisons, the molecular weight distribution of butene-based LLDPE often exhibits a narrower shear-thinning envelope than high-density grades because the target melt flow rate is reached at a lower molecular weight. During rotational moulding, this translates into a lower zero-shear viscosity and more rapid bubble release after densification. However, the narrower distribution can also produce a sharper melting front; operators should not use melt flow rate alone to predict oven dwell. Capillary rheometry at low shear rates, or small-amplitude oscillatory shear testing under ISO 6721-10, provides better correlation with rotomoulding performance than ISO 1133-1:2022 data alone.
On a three-arm carousel rotational moulding machine with a 3.2 m swing and through-the-wall thermocouples, powder densification for this density class begins when the internal air temperature reaches approximately 120–135 °C, and full consolidation of a 5 mm wall is usually complete between 185 °C and 200 °C. Peak internal air temperature is a more reliable release indicator than oven timer alone. The grade tolerates peak internal air temperatures of 200–210 °C without rapid surface oxidation; excursions above 230 °C consume antioxidant protection and increase inner-surface carbonyl index, leading to premature embrittlement. Production-scale trials with complex tool contours show that the 4.5 g/10 min melt flow rate fills narrow ribs and textured surfaces without excessive cycle extension, but under-densification can still occur where mould sections trap air or where powder bridging prevents contact with the heated wall.
Specification screening usually begins with density and melt flow rate because these two values bracket article stiffness, low-temperature ductility, and cycle economics. At 0.935 g/cm³, Icorene 3545 BUE 5524 provides a flexural modulus in the range of 650–750 MPa under ISO 178, which is typically 15–25% below the flexural modulus of a 0.945–0.950 g/cm³ medium-density rotomoulding powder. The trade-off is a measurable increase in sub-zero impact and a reduction in brittle failure from stress concentrations. The melt flow rate of 4.5 g/10 min is high enough to reduce cycle time in thin-wall parts, but low enough to avoid the pinhole and thin-out defects associated with rotomoulding resins above 6 g/10 min.
| Property | Representative range or value | Test method |
|---|---|---|
| Nominal density | 0.935 g/cm³ | ISO 1183-1:2019 |
| Melt flow rate | 4.5 g/10 min | ISO 1133-1:2022, 190 °C/2.16 kg |
| Tensile stress at yield | 17–20 MPa | ISO 527-2 |
| Tensile strain at break | >700% | ISO 527-2 |
| Flexural modulus | 650–750 MPa | ISO 178 |
| Environmental stress crack resistance | >1000 h | ASTM D1693 Condition B, 10% Igepal, 50 °C |
For powder handling, the material must be ground to a particle-size distribution compatible with the mould surface detail and heat-transfer rate. Coarse particles above 500 µm can leave unmelted inclusions or bubbles in thin walls, while excessive fines below 150 µm increase dust and reduce bulk flow from feed hoppers. Typical rotomoulding powders in this density class are supplied with controlled bulk density above 0.30 g/cm³ and low moisture content; the release documentation should be checked for volatiles, because moisture released during heating forms internal voids. Static charge and moisture control are more important when the powder is conveyed or dry-mixed with pigments or regrind.
Cooling rate determines final part dimensions and locked-in stress. Rapid water-spray cooling of the mould exterior sets the outer surface before interior crystallization is complete, reducing total shrinkage but increasing the risk of surface strain and warpage. Slower ambient cooling produces a more uniform crystalline population and lower thermal stress, at the cost of greater total shrinkage. For this LLDPE density class, expected demould shrinkage is generally in the 2.0–3.0% range when measured after 24 h of conditioning at 23 °C; local wall-thickness variation can push localized shrinkage outside that band and produce sink marks over bosses or ribs.
Outdoor rotomoulded parts made from unstabilized linear low-density polyethylene tend to fail first through surface chalking, micro-cracking, and loss of impact. The 5524 ultraviolet stabilization package in this grade is formulated to suppress photo-oxidative chain scission by a combination of UV absorption and radical scavenging. Under accelerated weathering in ISO 4892-2 or ASTM G155, stabilized LLDPE grades of this type retain a greater fraction of original elongation than unstabilized controls, although published data for this specific configuration is limited. For parts intended to exceed 10 years of rural or coastal exposure, accelerated weathering must be paired with natural exposure in the actual service climate because tie-chain degradation, pigment fade, and tensile loss do not always extrapolate linearly from xenon-arc hours. The stabilizer package is not a substitute for black pigments or coatings where UV screening is critical; for white or light-colored parts, a separate opaque pigment layer or co-moulded surface may be required.
In comparison with high-density polyethylene rotomoulding powders, Icorene 3545 BUE 5524 provides higher elongation and better low-temperature ductility because the lower density leaves a larger amorphous fraction and greater tie-chain capacity. In comparison with octene-based LLDPE rotomoulding grades, the butene-based BUE architecture reduces the ultimate impact and long-term ESCR at equivalent density and melt flow rate. The grade therefore occupies an intermediate position: it improves low-temperature impact relative to MDPE/HDPE while accepting moderate stress-crack resistance below that of octene LLDPE or cross-linked PE. This trade-off is relevant when specifying large containers with moderate hydrostatic load, complex shapes requiring good powder flow, or UV-stabilization needs at a controlled resin cost.
Regrind handling in rotomoulding with this grade requires particle-size control because ground scrap can degrade through chain scission and surface oxidation. Repeated heating and grinding cycles reduce tensile strain at break and increase the melt flow rate. Production lines that blend more than 20% regrind into virgin powder should monitor melt flow rate shift and impact loss; published data for this specific regrind blend ratio is limited, but the powder’s melt flow rate can act as a sensitive indicator of accumulated thermal degradation. If melt flow rate rises by more than 0.5 g/10 min relative to virgin reference, the blend may require revalidation for impact and ESCR.
For incoming quality assurance, oxidative induction time under ISO 11357-6 at 200 °C provides a faster check of the stabilizer package than full weathering. A low OIT value indicates antioxidant consumption during processing or storage. The measured OIT of a stabilized rotomoulding grade is not a direct service-life prediction, but it is a useful lot-to-lot consistency screen. Resin stored in hot or humid conditions should be rechecked before use, especially if packaging has been opened for extended periods.
| Requirement | Standard or regulation | Application scope |
|---|---|---|
| Olefin polymer food-contact compliance | FDA 21 CFR 177.1520 | Food-contact resin basis |
| EU plastic food-contact compliance | EU Regulation 10/2011 | Overall migration and SML |
| Accelerated weathering | ISO 4892-2 | Xenon-arc exposure |
| Chemical immersion | ISO 175 | Service-fluid compatibility |
| Melt flow rate QC | ISO 1133-1:2022 | Incoming resin verification |
| Density QC | ISO 1183-1:2019 | Incoming resin verification |
For potable-water tanks and packaging applications, compliance must be verified on the final article, not assumed from the resin grade. The rotomoulding process itself can generate oxidation products at the inner surface if peak internal air temperature is excessive, so a food-contact certification based on pellet or powder testing does not automatically cover the moulded surface. The final part may also require NSF/ANSI 61 testing for potable-water contact, and any pigment, mould release, regrind, or post-mould trimming operation must be included in the compliance review.
Pigmentation with dry organic pigments can alter rotomoulding behavior by acting as nucleating agents or by changing powder flow. In lightly colored parts, the UV stabilizer package must still be present in the base resin because many organic pigments do not provide adequate UV screening. For black parts, carbon black at 2–3% by mass is typically used as a UV absorber; the base stabilization remains necessary to protect thin-wall edges.
In field service, the main processing failure modes are under-densification pinholes along narrow ribs, inner-surface oxidation from over-curing, and warpage from asymmetric cooling. These failures are process-related rather than polymer-related, but they interact with the resin’s melt flow rate and stabilizer package. The grade is not recommended for continuous contact with aromatic hydrocarbons, strong oxidizing acids, or chlorinated solvents; the linear low-density polyethylene matrix absorbs certain organic solvents and loses mechanical strength by swelling. Immersion testing under ISO 175 with the actual service fluid is required before tank design is frozen. For chemical environments that exceed the resin’s ESCR or swelling limits, a cross-linked high-density polyethylene or a fluoropolymer-lined system should be specified instead.