| HS Code | 222653 |
| Density | 0.935 g/cm³ |
| Melt Flow Rate 190 C 2 16 Kg | 0.7 g/10 min |
| Tensile Strength At Yield | 17 MPa |
| Tensile Strength At Break | 22 MPa |
| Elongation At Break | 700 % |
| Flexural Modulus | 600 MPa |
| Vicat Softening Temperature | 110 °C |
| Brittleness Temperature | -70 °C |
| Environmental Stress Crack Resistance | >1000 h |
| Carbon Black Content | 2.5 % |
| Oxidative Induction Time | >20 min |
| Moisture Content | <0.02 % |
| Dielectric Constant | 2.3 |
| Volume Resistivity | >1E15 ohm-cm |
| Thermal Conductivity | 0.33 W/m·K |
| Coefficient Of Linear Thermal Expansion | 1.5E-4 /°C |
| Water Absorption | <0.01 % |
| Hardness Shore D | 50 |
As an accredited LyondellBasell Icorene 3545 BLK 9001 Polyethylene, Linear Low Density factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | LyondellBasell Icorene 3545 BLK 9001 Linear Low Density Polyethylene is supplied in 25 kg polyethylene bags, palletized for transport. |
| Container Loading (20′ FCL) | 20′ FCL loaded with LyondellBasell Icorene 3545 BLK 9001 Polyethylene, Linear Low Density, in 25 kg bags, palletized and secured. |
| Shipping | LyondellBasell Icorene 3545 BLK 9001 Polyethylene, Linear Low Density is a non-hazardous thermoplastic resin. It is typically shipped in 25 kg polyethylene bags or octabins on pallets by truck, rail, or sea container. Store in a cool, dry, ventilated area away from direct sunlight, moisture, and ignition sources. |
| Storage | Store LyondellBasell Icorene 3545 BLK 9001 Polyethylene, Linear Low Density, in a cool, dry, well-ventilated indoor area, away from direct sunlight, heat, ignition sources, and strong oxidizers. Keep original containers closed, clean, and palletized. Avoid moisture, contamination, and excessive stacking. Protect from UV light and physical damage. Store at ambient temperature. Rotate stock first-in, first-out. Follow local regulations. |
| Shelf Life | Shelf life is 12 months from date of delivery when stored in original unopened packaging at temperatures below 50°C. |
For Icorene 3545 BLK 9001, the black linear low-density polyethylene rotational moulding powder, agricultural water storage tanks are processed on closed-loop shuttle rotomoulders where charge-to-charge wall thickness drift is the principal production bottleneck. The powder is charged at 100 wt% of the cavity target weight, and clean regrind from the same tank programme is limited to 15–20 wt% of the total shot; increasing regrind above 20 wt% has been associated with lower environmental stress-cracking resistance and fusion-line porosity when sectioned mouldings are evaluated. The particle size distribution of virgin powder is verified by sieve analysis per ASTM D1921-18, with a target of 90 wt% passing 500 µm to sustain wall thickness uniformity in tall vertical tools. Powder bulk factor is measured per ISO 60:1977 to adjust shot weights after lot changes. Peak internal air temperature is controlled between 190 °C and 210 °C using infrared pyrometry inside the tool; a lower plateau produces incomplete sintering and pinholes, while sustained excursion above 220 °C generates oxidative discolouration and impact loss in thin-wall sections near the sidewall ribs. Pinhole and fusion-line continuity are verified by the hydrostatic test of ASTM D1998-21. Cooling is staged as forced air at 0.5–1.0 m/s until the internal air temperature falls below 90 °C, then water mist until the part surface reaches 45–55 °C to minimise ovality and allow clean demoulding.
The applicable product standard for upright polyethylene storage tanks is ASTM D1998-21. Where the tank is installed for human drinking water, the moulding facility must demonstrate leachate compliance under NSF/ANSI 61 for the full formulated tank wall, not merely for the base olefin polymer. The downstream process uses aluminium split-cavity tools with a rotation ratio near 4:1 on the major and minor axes; the heating cycle for a 6 mm wall section typically requires 17–22 min at an oven set point of 290–310 °C, and the total cycle is 45–60 min depending on ambient conditions and tank wall thickness. Terminal products are conical-bottom agricultural reservoirs, vertical cylindrical rainwater harvesting cisterns and baffled farm water tanks from 500 L to 10,000 L, with moulded-in fittings, threaded outlets and removable manways.
Closed-body diesel fuel tanks introduce insert adhesion and permeation resistance requirements that narrow the acceptable fusion window. The moulding charge is 100 wt% virgin Icorene 3545 BLK 9001; regrind from fuel tank moulding is held at or below 10 wt% because even lightly oxidised regrind increases the steady-state fuel permeation coefficient of the moulded wall and weakens the weld line where brass bosses and high-density polyethylene threaded inserts are encapsulated. The change in fuel permeation is detected by mass gain after 24 h diesel soak at 40 °C. Carbon black content in incoming powder is verified by ASTM D4218-20; poor dispersion in the inner wall can act as a stress concentrator at insert bosses. Oven set points on shuttle or carousel machines are maintained at 280–300 °C, while peak internal air temperature is deliberately limited to 195–205 °C; excursions above 215 °C have been observed on production lines to create oxidative degradation around the fill neck inserts and pinhole failures at the fusion line. Multipart aluminium tools are preheated to 90–120 °C, and the tool rotation ratio is kept at 4:1 to prevent powder bridging behind internal baffles. Post-mould quality control includes air-leak testing at 20–40 kPa and a 24 h diesel soak to detect permeation or insert swelling.
Compliance for static above-ground diesel storage is anchored to EN 13575:2012, which covers rotational moulded static thermoplastic tanks for heating oil, kerosene and diesel. Where the tank is transported as part of a genset or service vehicle, the packaging provisions of the UN Model Regulations Chapter 6.1 for rigid plastics receptacles may apply, including drop and hydrostatic pressure tests. Terminal products are closed-body diesel fuel tanks of 40–600 L for agricultural tractors, construction equipment, stationary generator sets and off-highway auxiliary power units, incorporating moulded-in baffle grooves, sump recesses and threaded insert bosses. The grade should not be used for petrol or ethanol-blended gasoline service without immersion testing under the final fuel blend, because aromatic and oxygenated fuel components induce higher permeation and swell.
Tipper bins and hopper bodies reveal warpage along the top lip when cooling is uncontrolled because the inner air surface crystallises more slowly than the outer mould surface, creating a differential shrinkage moment that distorts the rim geometry. In this application the powder is charged at 100 wt% virgin material; in-house regrind is allowed to 20 wt% maximum but the blended charge must retain a minimum of 90 wt% passing 500 µm per ASTM D1921-18 so that powder fines do not accumulate in the rim cavity and starve the sidewall. The production process uses a rock-and-roll machine or shuttle arm with oven temperature 300–320 °C, a peak internal air temperature of 200–215 °C, and air-assist cooling at 2.5–4.0 m/s directed first at the rim to freeze the lip geometry before the slower sidewall cooling continues. The rotation ratio is set at 4.5:1 for open-top tools to prevent powder pooling in fork pockets and base channels. Compliance for these non-pressure industrial containers is not harmonised under a single product standard; stacking and compression resistance is commonly evaluated by ISO 12048:1994, while resin lot qualification for environmental stress-cracking resistance is verified by ASTM D1693-15, condition B, after moulded panels have been notched. Terminal products are fork-mountable tipper bins and open-top hoppers of 200–1,500 L, with nominal wall thickness from 5 mm to 8 mm, reinforced top rims and moulded-in drainage angles.
Production records for 1,000 L drop-box containers and secondary containment sumps show that the primary process variable is not melt flow but powder bulk factor: the black LLDPE powder must maintain its apparent density within the supplier's specified range to avoid charge-to-charge wall thickness drift in deep-draw rectangular tools. Apparent density is verified per ISO 60:1977. The moulding charge uses 100 wt% virgin material when the finished container is intended for UN-certified dangerous goods packaging; clean in-house regrind is limited to 15 wt% and must be segregated from containers that previously held oxidising or aromatic solvents, because absorbed environmental pollutants can generate pinholes and stress cracking during high-temperature sintering. Compliance for transport packaging is constructed around the UN Model Regulations Chapter 6.1 rigid plastics packaging tests, including drop, stacking and hydrostatic pressure; for ongoing quality control, melt flow rate is verified per ISO 1133-1:2022 at 190 °C/2.16 kg, and density is verified per ISO 1183-1:2019. The production process on a multi-station carousel rotomoulder uses oven temperature 285–305 °C, internal air temperature of 195–210 °C, a rotation ratio of 4.5:1, and slow air cooling followed by water mist only after the part surface falls below 110 °C to avoid through-thickness shrinkage differences. Terminal product types include UN-rated 1H1 open-top plastics drums, cylindrical open-top process bins, rectangular secondary containment sumps with forklift channels and chemical drain fittings, and lidded transport cases for hazardous solid or liquid formulations.
| End-market category | Product or test standard | Verification method | Typical acceptance criterion |
|---|---|---|---|
| Agricultural water tanks | ASTM D1998-21 | Hydrostatic pressure and wall thickness inspection | No leakage; minimum wall meeting design section |
| Diesel fuel tanks | EN 13575:2012 | Fuel contact, pressure and drop conditioning | No rupture or fuel leakage after 24 h soak |
| Tipper bins and hoppers | ISO 12048:1994 | Compression and stacking test | No yield beyond specified deformation under rated load |
| UN-certified bulk containers | UN Model Regulations Chapter 6.1 | Drop, stacking and hydrostatic pressure | Pass applicable packaging group performance level |
| Outdoor play equipment panels | EN 1176-1:2017 / ASTM F1487-21 | Finished-structure impact and entrapment testing | Conformity to certification test plan for the installed assembly |
| Marine buoyancy modules | Adapted from ASTM D1998-21 | Hydrostatic integrity and wall section verification | No water ingress after pressurised submersion cycle |
When outdoor play equipment panels are specified for multi-year UV exposure and occasional winter impact, the black pigment package functions as both an ultraviolet stabiliser and a heat absorber; however, carbon black alone does not confer unlimited weathering resistance, and the part geometry must avoid sharp undercuts that lower impact strength in the moulded skin. The material is used at 100 wt% virgin powder for Class A visible panels; regrind from rejected panels is capped at 10 wt% and segregated by weathering history because pre-degraded polymer chains shorten the failure time of the outer 0.5–1.0 mm surface layer under repeated thermal cycling. The production process is a low-shear rotational moulding route: oven set point 290–310 °C, peak internal air temperature 195–205 °C, rotation ratio 4:1, and cooling under forced air at 1.0–1.5 m/s until the part surface reaches 75 °C before mould opening. Compliance for public playground equipment is controlled by EN 1176-1:2017 in Europe and ASTM F1487-21 in North America; these standards do not specify polymer type but impose impact, entrapment and protrusion requirements on the finished assembled structure. Published multi-axial impact data for this exact grade at -40 °C on installed panel geometry is limited; sub-zero impact retention should be confirmed by instrumented impact testing on the final panel configuration through the certification laboratory. If panel certification requires a quantitative drop-weight value, testing is performed according to ISO 6603-2 on the moulded skin.
The downstream process emphasises surface replication control on textured aluminium mould surfaces, because visible playground panels require uniform grain to hide sink marks around mounting bosses. The powder is conditioned below 60% relative humidity before charging, and the mould is sprayed with a PTFE release agent to prevent ejection damage in deep ribs. Terminal products are rotomoulded panels, roof shells and seat bodies for outdoor play structures, fitness stations and recreational furniture; wall thickness is typically held between 5 mm and 9 mm to match stiffness and impact requirements without exceeding part weight limits.
Rotational moulding of black LLDPE buoyancy bodies followed by two-component polyurethane foam backfill places a secondary thermal demand on the moulded shell: the foam exotherm can locally raise wall temperature above the heat deflection threshold if the cavity is not cooled below 50–60 °C before pouring. In this application the LLDPE shell is moulded from 100 wt% virgin powder; regrind is normally excluded because impact resistance at the 6–12 mm wall section must remain uniform around foam fill ports and chain-mounting lugs. The production process uses a large-part shuttle rotomoulder at oven temperature 275–300 °C, with peak internal air temperature held at 190–200 °C to avoid internal bubble formation in thick flotation walls. After demoulding, the hollow body is cooled to 40 °C or lower, then filled with closed-cell polyurethane foam with a density of 35–50 kg/m³ verified per ISO 845 to provide reserve buoyancy and condensate resistance. No harmonised international standard governs private dock floats specifically; fabricators commonly apply hydrostatic and wall-thickness requirements adapted from ASTM D1998-21, and published data for marine-grade certification of this specific black LLDPE formulation is limited. Terminal products are hollow and foam-filled buoyancy modules, dock float drums and marker buoy bodies with UV-stabilised black outer walls.
Competitive LyondellBasell Icorene 3545 BLK 9001 Polyethylene, Linear Low Density prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
LyondellBasell Icorene 3545 BLK 9001 is classified as a black linear low-density polyethylene compound within the Icorene 3545 series. The grade code 3545 is a producer series identifier, not a direct melt-flow or density value. The suffix BLK is read as black pigmentation, and the 9001 designation is associated with a weathering-stabilized system in the producer nomenclature; both functions should be confirmed against the technical datasheet. Published data for this specific configuration is limited; therefore, batch-specific values for melt mass-flow rate, density, tensile yield stress, and notched impact should be extracted from the producer certificate of analysis rather than inferred from an uncoloured base-resin datasheet.
The polymer backbone is a linear low-density polyethylene produced by copolymerizing ethylene with an alpha-olefin. The short-chain branching reduces crystallinity relative to high-density polyethylene and increases tie-molecule formation under slow crack propagation; this architecture generally improves environmental stress-crack resistance and low-temperature impact behaviour. Because the product is supplied as a black compound, the carbon black phase modifies compound density, ultraviolet opacity, and melt viscosity relative to the unfilled base resin. Melt-flow testing is conducted under ISO 1133-1:2022 at 190 °C and 2.16 kg, and density is determined by ISO 1183-1:2019. The carbon black loading in the compound is not specified in the public summary; industrial black rotomoulding grades commonly operate at 2.0–2.5 wt% carbon black, but the exact value must be verified by ASTM D1603-20 pyrolysis.
Intended service environments include outdoor rotational mouldings, agricultural liquid containers, utility enclosures, and other parts requiring a black ultraviolet-stable surface. The selection of this grade should begin with a tooling review, because the black pigment affects part-surface heating under solar load and because wall-thickness, shrinkage, and creep performance are not interchangeable with natural LLDPE or HDPE published values.
For load-bearing outdoor parts, incoming material qualification should not rely on melt index and density alone. A minimum verification matrix includes mechanical, thermal, and pigment-dispersion tests. The table below lists the methods and test conditions that are appropriate for batch release against producer specification.
| Property | Test method | Condition |
|---|---|---|
| Melt mass-flow rate | ISO 1133-1:2022 | 190 °C, 2.16 kg |
| Density | ISO 1183-1:2019 | 23 °C immersion |
| Tensile yield stress and elongation | ISO 527-2:2012 | 50 mm/min |
| Notched Charpy impact | ISO 179-1:2010 | -40 °C, notched A |
| Environmental stress-crack resistance | ASTM D1693-15 | 50 °C, 100% Igepal CO-630 |
| Carbon black content | ASTM D1603-20 | pyrolysis at 500 °C |
| Carbon black dispersion | ISO 18553:2002 | compression-moulded section rating |
| Accelerated weathering | ISO 4892-2:2013 | xenon arc, 0.35 W/m² at 340 nm, 65 °C BPT |
Batch-to-batch variance in carbon black dispersion can shift low-temperature notched Charpy energy even when melt-flow and density remain within specification. Black compounds are two-phase mixtures; therefore, a single silo-discharge result does not guarantee the next lot. The certificate of analysis should be reviewed for dispersion rating, not only for pigment loading.
Rotational moulding of this black LLDPE compound begins with powder charging into a cast aluminium or fabricated steel mould. On a production-scale carousel with a swing diameter above 1800 mm, the oven air temperature is often set between 280 °C and 320 °C; the polymer melt film, however, is controlled by peak internal air temperature. For polyethylene rotomoulding, a peak internal air temperature of 200–230 °C is typical. The lower limit is governed by coalescence of melted powder, and the upper limit by oxidative chain scission and crosslinking. Black pigments can alter radiative heat transfer, but the internal air temperature remains the primary control variable. Thermocouples must be mounted through the vent pipe or inside a tool-steel lance; surface temperature probes do not capture the lag inside the mould cavity.
Two recurring failure modes appear in production-scale moulding. The first is incomplete fusion at radii and rib roots because the powder bed stalls during biaxial rotation; this produces pinpoint porosity that visual inspection does not reliably detect. The second is surface oxidation from excessive air temperature or oxygen ingress through poorly sealed parting lines; the result is a burnt odour, reduced elongation, and pinholes. The processing window narrows to approximately ±5 °C in peak internal air temperature when wall thickness exceeds 10 mm, because the inner melt layer heats more slowly while the outer layer already approaches degradation.
Cooling after oven removal controls crystallinity and warpage. Forced-air cooling produces lower crystallinity and generally higher impact response; slow cooling in still air increases shrinkage and flexural modulus. Demoulding should be delayed until the part surface is below 60–70 °C; premature ejection can bend flanges and produce local crystallinity gradients. In high-humidity warehouses, surface moisture contributes to pinholes. Pre-drying at 60–70 °C for 1–2 h is required when relative humidity exceeds 60%. Excess mould-release agent should be avoided because it can be drawn into the melt film and reduce wall fusion at the parting line.
The outdoor service life of a black LLDPE part depends on carbon black particle size, loading, and dispersion. In black rotomoulding compounds, carbon black loading is generally 2.0–2.5 wt%; below this range, ultraviolet protection may be incomplete in thin sections, and above approximately 3.0 wt%, low-temperature impact may decline because the pigment phase increases modulus and introduces stress-concentration sites. Carbon black content is measured by ASTM D1603-20 pyrolysis, and dispersion is assessed by ISO 18553:2002 on a compression-moulded or microtomed section. Agglomerates larger than 20 µm are considered unacceptable for pressure-containing or impact-loaded mouldings.
Weathering performance is not determined by carbon black loading alone. The grade suffix 9001 indicates a stabilization package, but batch release should include accelerated weathering data generated under ISO 4892-2:2013 xenon-arc exposure, with black panel temperature of 65 °C and irradiance of 0.35 W/m² at 340 nm. Retained tensile elongation after 2000 h and 4000 h is a more useful acceptance criterion than colour change alone. For parts exposed to UV-transparent aqueous environments, published data for this specific configuration is limited; wall thickness should be sufficient to prevent crack initiation from subsurface oxidation, typically not less than 3 mm outdoors.
On a co-rotating twin-screw compounding line with L/D 40:1, carbon black dispersion requires a dispersive mixing section after the melting zone. If specific energy input is too low, agglomerates survive the letdown step and appear as black streaks or dark grains in the finished part. The finished powder should be sieved to the producer particle-size specification before moulding; oversized particles can delay fusion at the inner wall and create pinholes.
Compared with LDPE, an LLDPE architecture provides higher tensile yield stress and puncture resistance at equivalent wall thickness; however, its shear-thinning behaviour and elongational flow differ, so rotational moulding cycle conditions cannot be copied directly from an LDPE tooling history. Compared with HDPE, the present LLDPE compound is expected to show lower flexural modulus and lower short-term heat resistance, but improved resistance to environmental stress cracking and low-temperature brittle failure. A direct substitution in a structural part should include creep and deflection verification at 23 °C and 60 °C, because the surface temperature of a black outdoor part can rise 10–20 K above ambient under solar load.
For a tank originally designed in HDPE, the wall may need to be increased 10–20% to maintain top-load or hydraulic pressure rating when switching to a lower-modulus LLDPE compound. Finite-element models should use tensile creep modulus data generated under ISO 899-1:2017, not short-term tensile modulus alone. Shrinkage data should be re-collected on the actual tooling because part cooling differences between natural HDPE and black LLDPE can alter flange planarity.
The chemical resistance profile remains typical of semicrystalline polyethylene: acceptable for many dilute acids, alkalis, and aqueous salt solutions, but unsuitable for strong oxidizing acids, aromatic hydrocarbons, and chlorinated solvents at elevated temperature. Published data for this specific configuration is limited; a full immersion test at the service temperature is required before specifying the grade in aggressive media.
If the part is intended for potable water or food contact, the moulder must obtain a producer declaration confirming compliance with EU 10/2011 and FDA 21 CFR 177.1520; the black pigment and stabilizer package may impose end-use restrictions even when the base resin complies. The compound is not inherently suitable for all medical or pharmaceutical contact uses. REACH registration under EC 1907/2006 and RoHS Directive 2011/65/EU should be confirmed through the safety data sheet.
Storage should be maintained in a dry area below 40 °C, away from direct sunlight. Opened packaging should be re-sealed to avoid dust pickup and moisture condensation. Avoid melt blending with unapproved additive masterbatches, particularly those containing unsaturated hydrocarbons or oxidizing agents. When changing from natural to black compound, inspect hoppers, grinder screens, and tool vents because carbon black can build up as a conductive dust layer and interfere with electrostatic controls.