| HS Code | 107711 |
| Manufacturer | LyondellBasell |
| Product Name | Icorene 1761 WHI 1006 |
| Polymer Type | Linear Low Density Polyethylene (LLDPE), Metallocene |
| Density | 0.917 g/cm³ |
| Melt Flow Rate | 1.0 g/10 min (190°C/2.16 kg) |
| Melting Point | 119 °C |
| Vicat Softening Temperature | 100 °C |
| Crystallization Temperature | 100 °C |
| Tensile Strength At Yield | 9 MPa |
| Tensile Strength At Break | 25 MPa |
| Elongation At Break | 600% |
| Flexural Modulus | 200 MPa |
| Hardness | Shore D 50 |
| Dart Drop Impact | 200 g |
| Coefficient Of Friction | 0.2 |
As an accredited LyondellBasell Icorene 1761 WHI 1006 Polyethylene, Linear Low Density, Metallocene factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | LyondellBasell Icorene 1761 WHI 1006 metallocene linear low-density polyethylene, white pellets, packaged in 25 kg bags on 1000 kg pallets. |
| Container Loading (20′ FCL) | Icorene 1761 WHI 1006 metallocene LLDPE resin in 25 kg bags, palletized, shrink-wrapped, loaded into a 20-foot FCL for export. |
| Shipping | LyondellBasell Icorene 1761 WHI 1006, a white metallocene linear low-density polyethylene, ships as non-hazardous pellets in 25 kg PE bags on stretch-wrapped pallets. Transport in dry trucks or containers, protected from moisture, heat, contamination, and direct sunlight. Store cool, dry; standard PPE recommended. No special UN hazard class required. |
| Storage | Store in a cool, dry, well-ventilated area. Keep containers tightly closed and protect from direct sunlight, heat, moisture, and contamination. Keep away from ignition sources, strong oxidizing agents, and incompatible materials. Minimize dust generation and static buildup. Use original packaging, maintain clean handling conditions, and follow the supplier’s safety data sheet and local regulations. |
| Shelf Life | 24 months from date of manufacture when stored unopened in a dry, cool place away from direct sunlight and odors. |
Typical trade literature places Icorene 1761 WHI 1006 among metallocene-catalyzed hexene LLDPE grades with nominal density near 0.918 g/cm³ and melt flow rate near 1.0 g/10 min when tested according to ISO 1133-1. Converter certificates of analysis should override trade values for lot-specific work. The application set below is limited to real downstream conversion routes for metallocene linear low-density polyethylene film and sheet structures.
Cast film lines processing Icorene 1761 WHI 1006 use a single-screw extruder with 30:1 L/D and a barrier screw cut for linear-low-density polyethylene. Melt temperature is maintained between 240 °C and 260 °C to suppress melt fracture at high output. Die gap is set from 0.8 mm to 1.0 mm. Chill roll temperature is held between 15 °C and 25 °C. Vacuum box or air-knife assist is required above 200 m/min to prevent web flutter and uneven draw. The narrow molecular weight distribution of the metallocene catalyst system reduces low-molecular-weight extractables in the finished web. Extractable performance is relevant for direct food contact under EU Regulation 10/2011 and FDA 21 CFR 177.1520. Film gauge is typically reduced to 12–25 µm where dart impact and seal integrity remain compliant. Pinhole formation becomes the controlling failure mode below 10 µm on high-speed vertical form-fill-seal lines. Film optical properties are measured by ASTM D1003 haze and ISO 2813 gloss. The grade may be dry-blended with C8 metallocene LLDPE at 10–30 wt% where surface haze must be adjusted without sacrificing seal strength. Published data for this specific configuration is limited; converter trials are required to validate extractable performance after corona treatment and solventless lamination.
For direct food contact, the converter must verify that the grade’s as-supplied additive package meets the specific migration limits of the intended food type. Melt temperature below 220 °C is not recommended on short-residence-time cast lines because unmelted polymer particles may form during rapid plastication. Screw speed and backpressure should be set to maintain a melt pressure above 120 bar at the screen changer. A screen pack of 60/80/100 mesh is commonly used to capture incidental contamination without excessive melt temperature rise. Gauge uniformity is controlled by a die bolt profile and automatic air-gap thickness scanning. The target gauge variation across the web should not exceed ±5% for stable draw resonance-free operation.
For heavy-duty sacks, the blown film bubble is run at a blow-up ratio of 2.2:1 to 2.8:1 with a die gap from 1.6 mm to 2.2 mm. Single-screw extruders with 30:1 L/D grooved feed sections and barrier screws are used. Melt temperature is held at 190–210 °C. Output rates on a 350 kg/h tower may reach 180–220 kg/h before bubble instability becomes limiting. The frost line height is maintained at 6–8 die diameters to balance film crystallinity and tear resistance. Bubble breathing may appear when the grade is run neat above 220 kg/h on narrow die lips. Blending with autoclave LDPE at 20–30 wt% restores bubble stability but reduces dart impact. The sack film is downgauged from 120 µm to 90 µm only after tear resistance and pinhole resistance are revalidated. Dart impact is measured according to ISO 7765-1. Elmendorf tear is measured according to ISO 6383-2. The limiting property is often machine-direction tear propagation, not tensile yield.
| Process variable | Cast film | Blown film | Extrusion coating |
|---|---|---|---|
| Melt temperature | 240–260 °C | 190–210 °C | 290–320 °C |
| Die gap | 0.8–1.0 mm | 1.6–2.2 mm | 0.6–0.8 mm |
| Draw ratio or blow-up ratio | 20:1–40:1 | 2.2:1–2.8:1 | coating weight 12–25 g/m² |
| Cooling condition | chill roll 15–25 °C | frost line 6–8 die diameters | chill roll 15–20 °C |
Extrusion coating lines replace autoclave LDPE skins with Icorene 1761 WHI 1006 only as a blend partner. The grade is added to autoclave LDPE at 20–40 wt%. Melt temperature is set between 290 °C and 320 °C to control draw resonance and edge neck-in. A 15 µm coating weight is achievable when the melt curtain remains stable across the die width. Edge neck-in must be measured against the die width on each run. Typical target for liquid packaging board lines is below 150 mm total neck-in at standard die widths. Published data for this specific configuration is limited. Converter trials are required because neck-in depends on die design, air gap, and melt temperature. Adhesion to paperboard is promoted by ozone treatment and corona discharge. The mLLDPE-rich skin may require a tie layer or adhesion promoter when extrusion is run at low melt temperature. Heat seal performance of the coated board is tested by ASTM F88 and ASTM F1921. Hot-tack strength is critical for aseptic sealing jaws. The mLLDPE component narrows the hot-tack window compared with LDPE-rich skins. Line speed is limited by web tension and chill roll release rather than melt strength alone.
Neat mLLDPE is not recommended for high-speed extrusion coating because of high neck-in and draw resonance. The wider die gap of 0.6–0.8 mm combined with a low air gap of 150–250 mm improves melt curtain stability. Chill roll surface finish is selected between gloss and matte depending on board release requirements. Backside adhesion and seal-through-contamination performance must be validated at the converter’s declared filling temperature. The grade contributes lower organoleptic transfer than some C4 Ziegler-Natta LLDPE grades. Residual polymer extractables remain subject to EU Regulation 10/2011 and FDA 21 CFR 177.1520.
Across three-layer cast pallet wrap lines, the core layer is compounded with Icorene 1761 WHI 1006 at 50–70 wt%. Skin layers carry polyisobutylene cling additive at 1.5–3.5 wt%. Total film gauge is regularly reduced to 12 µm on high-output cast lines running above 400 m/min. Pre-stretch ratio in the application equipment is set between 250% and 350%. Cling force is measured according to ASTM D5458. Tensile elongation in machine direction is measured according to ASTM D882. Puncture resistance is measured according to ASTM D5748. The grade’s hexene comonomer distribution contributes to high machine-direction elongation without excessive transverse-direction shrinkage. Film roll hardness must be controlled by adjusting winding tension. Hard roll defects increase noise and cling transfer on automatic pallet wrappers. Winding tension is set lower than for conventional C8 Ziegler-Natta LLDPE because the mLLDPE core develops more contact clarity and surface tack after cooling.
Melt temperature in the cast line is kept between 240 °C and 245 °C to preserve cling additive in the skin layers. Higher temperature volatilizes low-molecular-weight polyisobutylene and reduces cling performance. The die gap is set at 0.8–1.2 mm for stable edge lay-flat. Chill roll temperature is held at 20–25 °C. Air knife pressure is adjusted to prevent air entrapment between film and chill roll. Excessive air entrapment creates optical defects that are measured as haze by ASTM D1003. The core mLLDPE layer permits downgauging from 17 µm to 12 µm only if puncture resistance remains above the end-user’s minimum threshold. That threshold is application-specific and should be fixed before commercial runs.
| Standard | Documentation requirement | Relevant limit or condition |
|---|---|---|
| FDA 21 CFR 177.1520 | Olefin polymer composition for food contact | Compliance subject to use conditions and food type |
| EU Regulation 10/2011 | Overall migration | 10 mg/dm² for general food contact |
| REACH SVHC | Candidate list substances | No intentionally added SVHC above 0.1% w/w |
| RoHS 2011/65/EU | Heavy metals and brominated flame retardants | Pb, Hg, Cr6+, PBB, PBDE 0.1% w/w; Cd 0.01% w/w |
Agricultural film lines exploit the narrow molecular weight distribution of the metallocene resin to produce three-layer cover film at total gauge from 150 µm to 200 µm. The core layer contains Icorene 1761 WHI 1006 compounded with hindered amine light stabilizer and UV absorber masterbatch at 8–15 wt% depending on exposure level. The two outer layers may contain EVA at 12–20 wt% to improve infrared retention and light transmission. Haze and light transmission are measured by ASTM D1003. Long-term weathering is evaluated by ISO 4892-2 xenon-arc exposure. The practical acceptance criterion is often tensile elongation retention after 3000 h of accelerated weathering. Published data for this specific grade under all stabilizer combinations is limited; the converter must run batch-specific weathering trials. The mLLDPE core improves the balance between puncture resistance and light transmission. Bubble stability on the agricultural blown film line is preserved by running at a blow-up ratio of 2.0:1 to 2.5:1. Frost line height is raised to 8–10 die diameters to promote film toughness. Melt temperature is held between 200 °C and 220 °C to limit additive degradation. Pre-drying of the UV masterbatch is required if storage relative humidity exceeds 60%. Uncontrolled moisture in the masterbatch produces gel defects and reduces film weather resistance.
Dust accumulation on greenhouse film remains a field limitation. The surface chemistry of the mLLDPE core does not eliminate dust adhesion. Anti-dust additives are incorporated into the skin layers where needed. This modification changes surface energy and may reduce film-to-film slip. The converter should measure coefficient of friction by ISO 8295 before high-speed tunnel lamination. Film blocking must be controlled by antiblock additive level. Antiblock addition reduces light transmission slightly. The operating window for the grade in this application is therefore set by the competing requirements of optical clarity, weather resistance, and winding performance.
In three-layer blown coextrusion for frozen seafood packaging, the sealant layer thickness is set at 12–18 µm to control seal-through-contamination performance. The substrate layers are formulated with higher-melt-strength LDPE or LLDPE to maintain bubble geometry. The sealant layer containing Icorene 1761 WHI 1006 is run at low melt temperature to preserve hot-tack performance. Hot-tack strength is measured according to ASTM F1921. Seal strength is measured according to ASTM F88. The usable seal initiation window is determined by the temperature at which the sealant layer reaches a minimum seal strength of 4 N/25 mm under the converter’s jaw pressure and dwell time. At storage temperatures of −20 °C, seal strength retention must be validated because ice crystals and fat contamination interfere with seal completeness. The low gel count of the metallocene resin improves seal continuity across the contaminated area. Gel defects above 200 µm are regarded as critical for this pack style. The grade is not used as the outer layer because surface toughness at freezer display temperatures is insufficient without a high-molecular-weight LLDPE or LDPE blend partner. Bubble stability is maintained with a blow-up ratio of 2.0:1 to 2.4:1. Frost line height is kept at 4–6 die diameters to maintain sealant layer clarity. Die gap is set between 1.4 mm and 1.8 mm. Output rate is limited by bubble sway on the upper tower. Published data for frozen seafood packaging using this exact grade is limited. Commercial adoption requires filling-line trials to confirm seal integrity under brine and ice contamination.
Competitive LyondellBasell Icorene 1761 WHI 1006 Polyethylene, Linear Low Density, Metallocene prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
LyondellBasell Icorene 1761 WHI 1006 is a white-pigmented metallocene-catalyzed linear low-density polyethylene supplied as pellets. The product identifier combines the base resin series Icorene 1761 with the colour package WHI 1006. The base resin is typically specified at a nominal melt-mass flow rate of 1.0 g/10 min at 190 °C/2.16 kg under ISO 1133-1:2022 and a nominal natural-resin density of 0.918 g/cm³ under ISO 1183-1:2019; the white pigmentation raises compound density relative to the natural polymer. Published product-specific mechanical data for the final white compound are limited in this document, and batch certificates of analysis must be used for acceptance testing.
The resin is used in monolayer and coextruded films where reduced seal initiation, downgauging capacity, optical uniformity, or a white opaque appearance is required. Typical application areas include food-packaging webs, frozen-food wrap, heavy-duty sacks, lamination films, and industrial liners. The metallocene catalyst produces a narrow molecular weight distribution and uniform α-olefin comonomer placement; this architecture separates the product from Ziegler-Natta linear low-density polyethylene, low-density polyethylene, and high-density polyethylene.
The replacement is controlled by molecular weight distribution. Ziegler-Natta LLDPE film grades commonly have Mw/Mn in the 3.5–5.0 range, whereas metallocene LLDPE grades are reported in the 2.0–3.5 range. The narrower distribution removes part of the high-molecular-weight tail and reduces shear thinning; consequently, melt viscosity at extrusion shear rates is higher than a Ziegler-Natta grade of equal melt-mass flow rate. On a 65 mm grooved-barrel extruder with a 30:1 L/D barrier screw and a 200 mm spiral mandrel die, the change can raise head pressure by 10–30% at constant screw speed and barrel set temperatures. The pressure increase is most acute when die gap is 1.5 mm or below, or when melt temperature falls below 200 °C. Thermal data for a hexene mLLDPE of the 0.918 g/cm³ class under ISO 11357-3 typically show a peak melting temperature near 121 °C, a crystallisation exotherm near 106 °C, and a Vicat softening temperature near 103 °C under ISO 306/A50. The white pigment package can shift crystallisation behaviour, so heat-seal and thermoforming set points must be verified on the actual compound.
In blown-film conversion, the first operational conflict is melt fracture from the narrow molecular weight distribution. Sharkskin onset for metallocene LLDPE is commonly observed at lower apparent shear stress than for Ziegler-Natta LLDPE; on a 1.2 mm die gap, the instability may appear between 200 s−1 and 400 s−1, depending on melt temperature and die-lip surface condition. The standard correction is to open the die gap to 1.8–2.5 mm, reduce throughput, or add a fluoropolymer processing aid at 200–800 ppm. If the film is intended for food contact, the processing aid must be cleared under FDA 21 CFR 177.1520 and EU Regulation (EU) No 10/2011. Because metallocene LLDPE lacks the long-chain branching of LDPE, bubble stability and melt strength are lower; a 10–20 wt% LDPE let-down is often used in high-stalk bubbles to suppress draw resonance. The exact ratio depends on cooling air velocity, die diameter, frost-line height, and the extruder’s screw-cooling capacity.
In cast-film conversion, the narrow molecular weight distribution can stabilise thickness variation at moderate line speeds; however, at draw ratios above 20:1 or melt temperatures below 220 °C, draw resonance may begin as periodic thickness bands. A smaller air gap of 15–25 mm and higher melt temperature are used to suppress the oscillation. The metallocene LLDPE may also require lower chill-roll temperature than Ziegler-Natta LLDPE to prevent blocking, and the coefficient of friction should be monitored under ISO 8295:1995 or ASTM D1894-14 after corona treatment.
When film thickness falls from 50 µm to 25 µm, dart impact becomes the limiting end-use property. Metallocene LLDPE retains impact better than Ziegler-Natta LLDPE at equivalent density because the uniform comonomer distribution raises the concentration of tie chains in the amorphous region. Dart impact is measured according to ISO 7765-1:2004 or ASTM D1709-16a, and the method energy range must be stated on the specification. Published comparative data for similar unpigmented 0.918 g/cm³ metallocene hexene LLDPE films indicate 30 µm blown-film dart impact values in the 800–1200 g range under method A, while 50 µm structures may exceed 1500 g. The white compound is expected to be lower because rigid pigment particles act as stress raisers; reductions of 10–20% relative to natural resin are not unusual. Tear properties under ISO 6383-2 or ASTM D1922-15 show orientation-driven anisotropy. High-stalk blown film usually has lower machine-direction tear than transverse-direction tear; the balance is adjusted through die gap, stalk height, frost-line height, and blow-up ratio.
In comparison with high-density polyethylene, the lower density of this metallocene LLDPE places it in the 0.918–0.920 g/cm³ class for the natural base resin, which lowers modulus and water-vapour barrier. Moisture-vapour transmission rate under ISO 15106-2 or ASTM F1249-20 is therefore higher than HDPE of 25–50 µm film thickness. Against LDPE, the metallocene LLDPE provides higher dart impact and tear resistance but lower melt strength in blow-up ratios above 3.0:1. In extrusion coating, this grade is not comparable to autoclave LDPE unless blended with LDPE to control neck-in and draw stability; the specific formulation must be evaluated on a pilot line of at least 200 mm die width.
For food-contact assessment, the olefin polymer component falls under FDA 21 CFR 177.1520 for olefin polymers, provided the conditions of use and food-type limitations are observed. In the European Union, the material must satisfy EU Regulation (EU) No 10/2011 as amended, including the overall migration limit of 10 mg/dm² and the applicable food-simulant testing for the intended contact time and temperature. The white pigment masterbatch must be included in the compliance assessment because TiO₂ surface treatment agents and organic processing aids can influence migration and organoleptic behaviour. For retort or sterilisation above 121 °C, the grade should not be assumed suitable without empirical validation under the actual pressure and package-headspace conditions.
| Property axis | Primary standard | Condition | Acceptance relevance |
|---|---|---|---|
| Melt mass-flow rate | ISO 1133-1:2022 / ASTM D1238-20 | 190 °C / 2.16 kg | Viscosity consistency and extruder pressure |
| Density | ISO 1183-1:2019 / ASTM D1505-18 | 23 °C immersion or gradient column | Film stiffness and barrier class |
| Tensile stress at yield | ISO 527-3:2018 / ASTM D882-18 | 500 mm/min for thin film | Load-bearing capacity |
| Dart impact | ISO 7765-1:2004 / ASTM D1709-16a | Method A or B; 25.4 mm dart | Puncture resistance in logistics |
| Elmendorf tear | ISO 6383-2:1983 / ASTM D1922-15 | Pendulum; single notch | Directional tear propagation |
| Haze | ISO 14782:1999 / ASTM D1003-13 | 0.5 mm specimen thickness | Optical clarity |
| Specular gloss | ISO 2813:2014 / ASTM D2457-13 | 45° geometry | Surface appearance |
| Coefficient of friction | ISO 8295:1995 / ASTM D1894-14 | 100 mm/min sled speed | Film converting and runnability |
Seal initiation is defined as the temperature at which seal strength reaches 2.0 N/25 mm under ASTM F2029-16. Relative to Ziegler-Natta hexene LLDPE of similar density and melt-mass flow rate, metallocene LLDPE may reduce seal initiation by 8–15 °C because the low-melting fractions are distributed more uniformly and no highly crystalline high-density fraction dominates the fusion interface. Hot-tack under ASTM F1921-18 measures the seal’s load-bearing capacity before crystallisation is complete. Metallocene LLDPE typically provides a broader hot-tack window because crystallisation is slower and more uniform; however, the white pigment increases the thermal mass of the film and may shift measured seal initiation by 2–5 °C. In vertical form-fill-seal operations above 40 m/min, dwell times below 0.5 s and jaw pressures from 2.0 bar to 6.0 bar require an empirical hot-tack curve. A set-point temperature that is not corrected for pigmented film thermal lag can produce leakers at the bottom seal; the corrective action is to run a seal-temperature map over the actual packaging line rather than relying on unpigmented films.