| HS Code | 247834 |
| Polymer Type | Metallocene Linear Low Density Polyethylene |
| Density | 0.917 g/cm³ |
| Melt Index | 1.0 g/10 min (190°C/2.16 kg) |
| Tensile Strength At Yield | 9.0 MPa |
| Tensile Strength At Break | 20.0 MPa |
| Elongation At Break | 800% |
| Flexural Modulus | 200 MPa |
| Vicat Softening Temperature | 93°C |
| Melting Point | 120°C |
| Hardness Shore D | 50 |
| Color | Red |
| Form | Pellets |
| Processing Method | Rotational Molding |
As an accredited LyondellBasell Icorene 1761 RED 4312 Polyethylene, Linear Low Density, Metallocene factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | LyondellBasell Icorene 1761 RED 4312 comes in 25 kg polyethylene bags, palletized and stretch-wrapped, with 1,000 kg per pallet. |
| Container Loading (20′ FCL) | 20′ FCL container loading for LyondellBasell Icorene 1761 RED 4312 metallocene linear low-density polyethylene; safely palletized and secured for transport. |
| Shipping | LyondellBasell Icorene 1761 RED 4312 is a non-hazardous metallocene linear low-density polyethylene resin. It normally ships in 25 kg bags, 1000 kg FIBCs, or bulk trucks/railcars, palletized and stretch-wrapped. Transport in clean, dry vehicles, protected from moisture, heat, and UV. No special hazard labels required. |
| Storage | Store LyondellBasell Icorene 1761 RED 4312 Polyethylene in a cool, dry, well-ventilated area away from direct sunlight, heat, sparks, and open flames. Keep original bags or containers tightly closed to prevent moisture, dust, and contamination. Avoid strong oxidizers. Use proper grounding to control static, protect from UV, and rotate stock. |
| Shelf Life | Shelf life is typically 24 months when stored unopened in original packaging, cool, dry, well-ventilated, away from direct sunlight. |
In the rotational moulding of chemical containment bunds and above-ground static tanks, the transition from Ziegler-Natta LLDPE to metallocene LLDPE changes the controlling failure mode at sub-zero temperatures. Moulded parts produced from Icorene 1761 RED 4312 are qualified under ISO 6603-2 instrumented puncture testing at −20 °C and ISO 179-1 notched Charpy at −18 °C; environmental stress-crack resistance is assessed under ASTM D1693-15e1 condition B in 10 % Igepal CO-630 at 50 °C. For above-ground storage of liquid fuels and chemicals, EN 13341:2005+A1:2011 governs static thermoplastic tank requirements. When the red tank is converted for potable water or food contact, FDA 21 CFR 177.1520(a) and EU 10/2011/EC Annex I overall migration limits must be verified on the finished rotomoulded wall, not inferred from natural-pellet data. The pigment package in the red 4312 formulation is evaluated for dispersion uniformity by reflected-light microscopy of microtomed sections at 200×; pigment agglomerates larger than 10 µm at the inner wall are treated as stress-concentration risks in chemical service.
Starting dry blend is 100 parts Icorene 1761 RED 4312, combined with 0.05–0.2 wt% phenolic/phosphite antioxidant and, for outdoor tanks, 0.3–0.8 wt% oligomeric HALS and 0.1–0.3 wt% UV absorber. No internal release agent is added at wall thickness below 8 mm; at 12–18 mm wall sections, a release agent allowance of 0.02–0.05 % may be used to reduce demoulding deformation, but it must be validated on baffle inserts because weld-line strength is reduced. Up to 10 wt% clean in-house LLDPE rotomoulding regrind from the same part family may be dry-blended into the powder; side-wall Charpy impact can decrease by approximately 4–7 % per 10 wt% regrind increment, so regrind is not used in the innermost chemical-contact layer where a uniform melt film is required.
Moulding is conducted on a biaxial rotational machine with a primary-to-secondary arm speed ratio between 4:1 and 5:1. Oven set points of 280–320 °C are used for double-wall tanks with 20–30 mm total wall thickness; peak internal air temperature is maintained at 190–210 °C for 15–25 min after reaching 150 °C, after which controlled cooling begins. Forced-air cooling from 190 °C to 100 °C at −8 to −12 K/min is followed by water-mist cooling to 60 °C to reduce flange warpage. Terminal parts are red chemical bunds, diesel spill sumps, dosing skid enclosures, and above-ground static tanks up to 10 000 L with moulded corner radii of 15–30 mm and no welding.
Clinical waste containers fabricated from red metallocene LLDPE are validated through transport-oriented performance testing rather than general-purpose melt-flow data. Drop testing is performed under ASTM D5276-19 at −18 °C and 23 °C on filled containers to simulate handling failures; puncture resistance is tested under ISO 6603-2 at −20 °C. Colour batch consistency is controlled by ASTM D2244-15e1 CIE Lab measurement with a tolerance of ΔE ≤ 1.5. For food-contact reuse of clean clinical logistics containers, migration is verified under EU 10/2011/EC Annex I and FDA 21 CFR 177.1520. The red shade itself is part of the hazard-coding system and must remain distinguishable after repeated steam cleaning at 121 °C for 15 min; surface colour is re-qualified after 50 simulated decontamination cycles.
Formulation uses 98–100 wt% Icorene 1761 RED 4312; the balance is a hindered phenol/phosphite stabilizer package at 0.05–0.2 wt% and, for containers stored outdoors before service, 0.2–0.4 wt% HALS. Fluoropolymer process aids are avoided because migration to gasket sealing surfaces reduces lid friction and compromises closure integrity; phthalate plasticisers are not used, aligning with EU 10/2011/EC and 21 CFR 177.1520 extractives requirements. If the powder has been exposed to ambient humidity above 60 % for more than 4 h, it is pre-dried at 60 ± 5 °C for 2 h before charging to reduce surface moisture defects on the lid gasket channel.
Rotational moulding is performed in matched cast-aluminium lid and base mould sets. Peak internal air temperature is set to 200–215 °C, with oven dwell of 25–40 min for 10–25 kg shot weights. Cooling between 120 °C and 80 °C is controlled at −10 to −15 K/min to maintain flatness of the gasket channel; steel lock handle inserts are preheated to 120 °C before mould charging to prevent cold spot cracking. Terminal products are red clinical waste bins, sharps containers, cytotoxic waste transport boxes, and pharmacy segregation bins with gasketed lids and metallic locking hardware.
| Segment | Standard/test method | Critical boundary |
|---|---|---|
| Chemical containment bunds | EN 13341:2005+A1:2011 | Peak internal air temperature 190–210 °C |
| Clinical waste containers | ASTM D5276-19 | Drop impact at −18 °C |
| Agricultural tanks | ISO 4892-2:2013 | Xenon-arc exposure 2 000–4 000 kJ/m² |
| Returnable logistics boxes | ISO 8611-1:2021 | Top-load compression after −20 °C impact |
| Marine fenders and floats | ISO 62:2008 | Water absorption at 23 °C for 24 h |
For agricultural crop protection equipment, the dominant ageing mechanisms are cyclical internal pressure from sprayer pumps, ultraviolet exposure, and contact with pesticide carrier liquids. Outdoor weathering is benchmarked using ISO 4892-2:2013 xenon-arc exposure of 2 000–4 000 kJ/m² at 340 nm; chemical resistance to liquid pesticides is evaluated under ISO 175:2010 immersion testing at 40 °C for 30 days. Oxidative stability of the stabilizer package is checked by oxidation induction time per ISO 11357-6:2018, with a minimum OIT of 20 min at 200 °C for exposed service. Because the tanks are red-pigmented and reach surface temperatures above 65 °C in direct solar load, stabilizer depletion is a more relevant failure mechanism than short-term tensile yield.
Dry-blend formulation is 100 parts Icorene 1761 RED 4312, 0.2–0.6 wt% oligomeric HALS, 0.1–0.3 wt% UV absorber, and 0–10 wt% clean in-house rotomoulding LLDPE regrind. The red pigment does not require additional wax dispersion at the stated volume, but dry-blend homogeneity is verified by total colour difference across three sampling points with ΔE ≤ 1.0. Metallocene LLDPE powder is not combined with high levels of external lubricant; if lubricant addition exceeds 0.05 wt%, the internal wall can develop low-gloss streaks and reduced chemical barrier uniformity, so exterior surface lubricants are preferred.
Rock-and-roll rotational machines handle cylindrical tanks from 20 L to 3 000 L; primary-axis speed is 8–12 rpm, secondary-axis speed 1.5–3 rpm, giving a speed ratio near 4:1. Peak internal air temperature is 190–205 °C, followed by forced-air cooling to 90 °C before water-spray cooling to 60 °C. Wall thickness is maintained at 5–10 mm; drain fitting inserts are beryllium-free aluminium to reduce galvanic corrosion. Terminal products are red agricultural sprayer tanks, pesticide mixing tanks, fertiliser hoppers, seed hoppers, calf feeding bowls, and vineyard frost-protection water containers.
Returnable logistics packaging compounded from Icorene 1761 RED 4312 is qualified under ISO 8611-1:2021 for pallet and bin racking loads, with top-load compression per ASTM D642-20 and repeated drop impact per ASTM D5276-19. Dynamic impact at −20 °C is the most discriminating requirement because the metallocene chain architecture reduces brittle failures relative to conventional LLDPE at the same wall section; however, the red pigment can mask early stress whitening, so impact damage is detected by tap testing rather than visual colour change. Food-contact bins, when used for post-consumer resin collection, are verified under EU 10/2011/EC and FDA 21 CFR 177.1520; industrial bins for non-food scrap are assessed for outdoor colour retention under ISO 4892-2:2013.
Formulation uses 85–95 wt% Icorene 1761 RED 4312 and 5–15 wt% HDPE with melt flow rate 4–8 g/10 min determined by ISO 1133-1:2022 at 190 °C and 2.16 kg. HDPE is dry-blended, not melt-compounded, to preserve rotational moulding powder flow; the higher HDPE fraction raises top-load rigidity but lowers notched Charpy impact in side-wall specimens by approximately 12–18 % at 15 wt% HDPE. Peak internal air temperature is extended by 3–5 min when HDPE is present so that the higher-melting fraction is fully sintered at the mould surface.
Clam-shell machines with 1 200 × 1 000 × 800 mm moulds and 8–15 kg shot weights use peak internal air temperature of 195–215 °C and oven dwell of 25–45 min. Cooling is staged: ambient air to 90 °C at −8 K/min, then water mist to 60 °C. Moulds include interlocking rib patterns with 3°–5° draft angles to reduce demoulding stress and permit clean ejection of undercut-free sidewalls. Terminal products are red pallet boxes, 1 200 × 1 000 mm logistics containers, automotive parts crates, and waste sorting containers for post-consumer plastic segregation.
In marine fender and buoyancy cell production, the absence of internal cavity pressure control shifts the process window to lower peak internal air temperature because red-pigmented metallocene LLDPE can show visible shade drift when heated above 210 °C for extended dwell. Material acceptance uses water absorption per ISO 62:2008 at 23 °C for 24 h, tensile properties per ISO 527-2:2012, Shore D hardness per ISO 868:2003, and low-temperature Charpy impact per ISO 179-1 at −20 °C. Published data for long-term saltwater immersion of this specific red 4312 formulation beyond 5 000 h is limited; therefore validation at 40 °C in artificial seawater according to ASTM D1141 is recommended for applications exceeding 18 months continuous immersion.
Formulation is 100 parts Icorene 1761 RED 4312 with 0.3–0.7 wt% HALS, 0.1–0.3 wt% UV absorber, and 0.05–0.2 wt% copper deactivator when the part is assembled with brass or copper mooring hardware. No external impact modifier is added because the metallocene architecture already provides low-temperature ductility; addition of EPDM or plastomer above 5 wt% is not required and can reduce Shore D hardness below 55, which is unacceptable for structural fender cores. No amine-based additive package is used because amine-catalysed oxidation by-products can accelerate discolouration of red marine parts during prolonged UV exposure.
Rotational moulding of thick-walled floats uses peak internal air temperature of 185–200 °C and oven dwell of 35–60 min for 15–40 kg parts. Cooling rate through the crystallisation range from 115 °C to 95 °C is limited to −5 to −8 K/min to maximise impact strength; faster cooling can reduce wall toughness by increasing quench-induced crystallite size gradients. Two-piece aluminium moulds with internal vent tubes avoid gas entrapment and permit foam filling after demoulding. Terminal products are red quay fenders, mooring buoys, flotation collars for dredge lines, and marker floats.
Competitive LyondellBasell Icorene 1761 RED 4312 Polyethylene, Linear Low Density, Metallocene prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
LyondellBasell Icorene 1761 RED 4312 is supplied as a metallocene-catalyzed linear low-density polyethylene rotomolding powder in a pre-colored red formulation. The base resin belongs to the Icorene metallocene LLDPE series; the numerical suffix 1761 identifies the melt-flow and density set point, while the RED 4312 designation identifies a specific red pigment package. For specification purposes, the relevant test methods are ISO 1133-1 for melt mass-flow rate at 190°C and 2.16 kg, and ISO 1183-1 for density. Published industrial data for metallocene rotomolding grades in this density class typically fall within 0.936–0.942 g/cm³ and 4.5–6.5 g/10 min; the actual nominal values for the pigmented product should be confirmed against the current LyondellBasell technical datasheet because the color concentrate can shift density and low-shear viscosity. Powder dry flow and bulk density are also controlled because these parameters govern mold charging, layer formation, and pinhole resistance; ASTM D1895 is commonly used for bulk density measurement.
In metallocene catalysis, the active sites are substantially uniform, which produces a narrower molecular weight distribution and a more homogeneous intermolecular and intramolecular comonomer distribution than multi-site Ziegler-Natta catalysts. The practical consequence in rotomolding is that impact toughness and environmental stress crack resistance can be retained at higher stiffness because the tie-molecule population is more uniformly distributed. Under ASTM D1693 Condition B, metallocene rotomolding grades in the 0.935–0.940 g/cm³ density range frequently exhibit F50 values exceeding 1000 h, while conventional Ziegler-Natta LLDPE grades of similar melt flow may fall below 500 h. Similarly, low-temperature impact testing to ISO 6603-2 at -20°C often shifts from brittle to ductile failure at lower wall thickness. The metallocene grade also has lower catalyst residues and lower hexane extractables, which is relevant for potable water and food-adjacent applications if the specific color package is cleared for those uses.
Rotational molding of Icorene 1761 RED 4312 is typically carried out on carousel, shuttle, or rock-and-roll machines with a primary-axis speed of 4–12 rpm and a secondary-axis speed of 1–4 rpm, producing a rotation ratio near 4:1. The powder is charged into aluminum or steel molds at ambient temperature, then heated in an oven with air setpoints between 260°C and 320°C. The critical control variable is internal air temperature, not oven setpoint; target peak internal air temperature for a metallocene LLDPE with density near 0.940 g/cm³ commonly falls in the 180–210°C range depending on wall thickness. Bubble removal and full densification require holding the polymer above the crystalline melting range for a defined plateau time. At wall thickness above 6 mm, cycle time is extended rather than increasing oven temperature excessively because thermal-oxidative degradation of the pigmented surface can occur. Thermocouple or infrared internal-air-temperature measurement is recommended to prevent pinhole defects, inner-surface roughness, and color shift.
The cooling segment after peak internal air temperature exerts a strong influence on part dimensions and impact performance. Cooling rates in the crystallization window below 2°C/min tend to increase spherulite size and post-mold shrinkage, while rates above 10°C/min can generate through-thickness thermal gradients that produce warpage and residual stress. Forced-air fan cooling is typically used for sections below 6 mm; water-mist cooling is restricted to thicker sections because rapid surface cooling can lock in internal voids or delaminate the inner skin. Dimensional stability should be checked after 24 h and 48 h post-demolding, as polyethylene continues to shrink through secondary crystallization. Warpage measurement can be performed using a granite surface plate and feeler gauges or laser scanning; no single pass/fail standard applies across all geometries, so correlation studies are required for each mold. The red-pigmented surface can reach peak temperature earlier in radiant-heat ovens than an unpigmented powder; operators should anticipate an oven setpoint reduction of 10–20°C or a shorter cycle time when transferring from natural to dark red material.
The RED 4312 suffix identifies a color concentrate, not a UV stabilization package or a regulatory certification. If the molded article is intended for outdoor service, the current technical datasheet and regulatory information sheet must be reviewed for the presence of hindered amine light stabilizers or ultraviolet absorbers. Accelerated weathering of red-pigmented polyethylene is commonly evaluated by ISO 4892-2 with black standard temperature, humidity, and irradiance settings specified per test duration. Color retention and impact retention after weathering should be measured by ASTM D2244 for color change and ISO 6603-2 for impact retention; published data for this specific pre-colored configuration is limited, so outdoor part qualification should not rely only on natural-grade data. For potable water or food contact, compliance under FDA 21 CFR 177.1520 or EU Regulation 10/2011 must be confirmed for the final colored compound, because pigments and processing aids may not be automatically covered by base resin clearances.
| Characteristic | Test method | Typical class envelope | Process or design significance |
|---|---|---|---|
| Density | ISO 1183-1, ASTM D1505 | 0.930–0.945 g/cm³ | Stiffness, permeation, and impact balance |
| Melt mass-flow rate | ISO 1133-1, 190°C, 2.16 kg | 3.0–8.0 g/10 min | Powder sinterability, bubble removal, and cycle time |
| Tensile stress at yield | ISO 527-2 type 1B | 12–20 MPa | Load-bearing design at ambient temperature |
| Flexural modulus | ISO 178 | 450–750 MPa | Panel stiffness and wall-section selection |
| Environmental stress crack resistance | ASTM D1693 Condition B, F50 | often > 500 h | Chemical container and tank service |
| Low-temperature impact | ISO 6603-2 at -20°C | Ductile mode in properly molded sections | Outdoor and cold-service toughness |
Compared with a conventional Ziegler-Natta butene LLDPE rotomolding powder of equivalent density 0.940 g/cm³ and melt flow 5.0 g/10 min, the metallocene grade generally provides higher puncture toughness, better environmental stress crack resistance, and lower extractables, while requiring tighter control of peak internal air temperature because of the narrower melting distribution. Compared with high-density polyethylene rotomolding powders in the 0.945–0.955 g/cm³ range, Icorene 1761 has lower stiffness and lower heat deflection temperature, but improved impact and ESCR. Compared with low-density polyethylene, the metallocene LLDPE offers higher tensile yield and better stress crack resistance while retaining adequate flow for large moldings. The pre-colored RED 4312 version differs from natural or UV-stabilized Icorene grades in that color dispersion is managed by the supplier, which reduces metering and dispersion variability on the shop floor but limits downstream color changes and may impose additional regulatory restrictions.
Production lines with regrind reprocessing should cap regrind at 20–30 wt% unless part testing demonstrates equivalent ISO 6603-2 impact and ASTM D1693 ESCR. Polyethylene is not hygroscopic, but surface moisture on powders stored at relative humidity above 60% can generate pinholes; drying at 70–80°C for 1–2 h in a desiccant or hot-air dryer is a standard preventive measure. When pigment masterbatch is produced on a co-rotating twin-screw extruder with L/D 40:1 and distributive mixing sections, dispersion quality influences impact retention; agglomerates larger than 10 µm can act as stress concentrators. The final powder is cryogenically ground, and sieve analysis is used to control particle size distribution because an excess of fines can reduce dry flow and increase dust, while coarse particles can produce uneven sintering.
Published data for the Icorene 1761 RED 4312 configuration is limited for some application-specific conditions, particularly long-term UV retention and potable water migration. Therefore, critical part qualification should include oven mapping, thermocouple-derived peak internal air temperature profiles, and mechanical testing on plaques molded under production-equivalent conditions. The use of antioxidant packages should be verified for the intended service temperature; continuous service above 60°C in aggressive chemical environments requires oxidative induction time testing to ISO 11357-6 or equivalent.