| HS Code | 635562 |
| Polymer Type | Polyethylene, Linear Low Density, Metallocene |
| Color | Red |
| Density | 0.917 g/cm3 |
| Melt Index 190 C 2 16 Kg | 1.0 g/10 min |
| Melting Point | 118°C |
| Vicat Softening Point | 93°C |
| Tensile Strength At Yield | 9.65 MPa |
| Tensile Strength At Break | 27.6 MPa |
| Elongation At Break | 750% |
| Flexural Modulus | 207 MPa |
| Hardness Shore D | 50 |
As an accredited LyondellBasell Icorene 1761 RED 4308 Polyethylene, Linear Low Density, Metallocene factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | LyondellBasell Icorene 1761 RED 4308: typically supplied in 25 kg moisture-resistant bags, 40 bags (1,000 kg) per pallet. |
| Container Loading (20′ FCL) | 20′ FCL: approximately 20,000 kg of LyondellBasell Icorene 1761 RED 4308 LLDPE metallocene resin, typically supplied in 25 kg bags. |
| Shipping | LyondellBasell Icorene 1761 RED 4308 is typically shipped as non-hazardous, red-pigmented metallocene LLDPE pellets in 25 kg bags or 1,000 kg bulk bags, palletized and stretch-wrapped. Transport in dry, covered trucks, railcars, or containers at ambient temperature, protecting from moisture, heat, and contamination. No special hazardous-materials handling required. |
| Storage | Store Icorene 1761 RED 4308 polyethylene in a cool, dry, well-ventilated area. Keep original containers closed and labeled, away from direct sunlight, heat, ignition sources, and strong oxidizers. Protect from moisture, dust, and contamination. Avoid static buildup; use grounding where required. Maintain ambient temperature and follow manufacturer SDS and local regulations. Do not store near food, drink, or incompatible materials. |
| Shelf Life | Shelf life is typically two years when stored in cool, dry, ventilated conditions away from direct sunlight in original packaging. |
LyondellBasell Icorene 1761 RED 4308 is supplied as a pre-coloured metallocene-catalysed linear low density polyethylene powder for rotational moulding. Before application-specific conversion, the incoming material is characterised under ISO 1133-1:2022 for melt flow rate, typically 3.5–6.0 g/10 min at 190 °C / 2.16 kg; under ASTM D1895-17 for bulk density, typically 0.31–0.35 g/cm³; and under ASTM D1921-18 for particle size distribution. Density of the final moulded wall is checked under ASTM D1505-18; nominal values for this mLLDPE class are 0.938–0.942 g/cm³. The useful particle fraction for rotomoulding is 250–600 µm, with fines below 250 µm limited to ≤10 % to avoid melt pooling in narrow rib sections. Oxidative induction time is measured under ASTM D3895-19; values below 20 min at 200 °C indicate antioxidant depletion and should not be released for thick-section tanks. Condensed moisture on cold powder is a more likely defect source than polymer hygroscopicity: bags stored at ≤50 % RH and 15–25 °C do not require drying before charging. Where outdoor storage has exposed the powder to humidity cycles above 70 % RH, a 4 h conditioning period at 40 °C in a vented hopper reduces bubble-related pinholes in 6.0 mm sections. The pigmentation itself alters infrared absorption; where the red colorant package includes iron oxide, the powder can reach peak internal air temperature 10–15 °C earlier than an identical natural powder on the same carousel cycle, so oven setpoints must be derived from line trials rather than historical natural-powder recipes.
| Downstream route | Primary compliance or test standard | Relevant property |
|---|---|---|
| Chemical secondary containment | EPA 40 CFR 264.175; ASTM D1998-21; EN 13575:2012 | Stress-crack resistance, full-volume containment |
| Agricultural sprayer tanks | ASTM D543-20; ISO 175:2010; ASTM D638-14 | Chemical resistance, tensile yield |
| Diesel exhaust fluid reservoirs | ISO 22241-1:2019; ISO 22241-2:2019; ISO 22241-3:2017 | Leachate control, urea purity retention |
| Marine buoyancy bodies | ASTM G154-16; ASTM D256-23 | Weathering retention, impact resistance |
| Bulk solids handling liners | ASTM D790-17; ISO 178:2019; ASTM D638-14 | Flexural modulus, tensile yield |
| UN-rated packagings | 49 CFR 178.603; ADR 6.1.5 | Drop, stack, and hydraulic pressure performance |
In chemical secondary containment sumps and dosing skid basins, Icorene 1761 RED 4308 is forced into the most severe stress-crack resistance demand of the conversion routes because stored fluids are rarely single-component and crack-accelerating surfactant residues are common in maintenance areas. The governing compliance set is EPA 40 CFR 264.175 for secondary containment capacity, ASTM D1998-21 for upright polyethylene storage tanks, and EN 13575:2012 for static thermoplastic tanks for above-ground service. The formulation boundary for this route is clean, same-lot regrind at no more than 20 wt%; if the stored fluid temperature exceeds 50 °C, regrind is reduced to 10 wt% and the antioxidant level is increased by 0.05 wt% through a pre-compounded masterbatch. On a multi-axis rock-and-roll machine with a 1,500–2,000 mm swing diameter and a 4:1 arm speed ratio, the red-pigmented powder reaches the target peak internal air temperature of 195–205 °C faster than natural powder; actual oven dwell for a 6.0 mm nominal wall is typically 34–42 min. A recurring production failure on this geometry is internal corner pinhole formation when powder sag leaves unfused particles in radii below 12.5 mm; increasing the part radius and capping PIAT at 205 °C reduces the pinhole rate below detection in sectioned trial parts. Terminal products are open-top chemical tanks, containment sumps, pump bases, and spill pallets with capacities from 110 L to 5,000 L. Oxidising agents above 5% active concentration and aromatic hydrocarbons above 25 wt% are outside the long-term service envelope of this material class unless a fluorinated barrier or compatible liner is specified.
When thin-wall agricultural sprayer tanks are converted from Icorene 1761 RED 4308, the dominant constraint shifts from long-term chemical exposure to cyclic flexure of walls below 4.0 mm and multi-season UV oxidation at the outer surface. The compliance baseline for the final tank is ASTM D543-20 and ISO 175:2010 for chemical resistance, with tensile acceptance under ASTM D638-14 and ISO 527-2:2012. In this route, a hindered amine light stabiliser concentrate is dry-blended at 0.15–0.30 wt% active HALS only when the certificate of analysis does not confirm a pre-compounded UV package; if acid-modified wetting agents are added in the same tumble, premature polymer oxidation during oven dwell can appear as surface yellowing and tensile elongation losses greater than 20%. The conversion process on a four-arm carousel machine with a forced-air oven uses an oven setpoint of 270–285 °C for the red powder, a peak internal air temperature of 190–200 °C, and water-mist cooling that is initiated only after the inner surface reaches 120 °C to avoid sink marks around moulded threads. Terminal products include saddle tanks, induction bowls, nurse tanks, and pump calibration cylinders from 40 L to 3,000 L. Published data for this specific red-pigmented mLLDPE grade in long-term glyphosate and urea–ammonium nitrate tank-mix exposure is limited; pre-production immersion tests at 40 °C for 90 days in the actual end-use fluid are required before tooling is released.
For diesel exhaust fluid service, the rotomoulded reservoir made from Icorene 1761 RED 4308 must not alter the urea solution conductivity or alkalinity beyond the purity limits of ISO 22241-1:2019 and the handling and storage provisions of ISO 22241-3:2017. The material leachate envelope is controlled by limiting regrind of the same red grade to 10 wt%; no external amide-based slip or antistatic additives are introduced because migration into urea solution increases insoluble residue and can fail the ISO 22241-2:2019 shelf-life stability assessment. Processing is performed on a shuttle-type rotational moulding machine with aluminium moulds and individual internal air temperature probes. The target PIAT is 190–198 °C, which is deliberately kept below the 200 °C upper limit used for natural mLLDPE because the red colorant package reduces the onset time for oxidative degradation at the outer wall. After demoulding, the inner surface is rinsed with demineralised water at 60 °C for 2 h and air-purged at 40 °C for 8 h to reduce leachable oligomers before first fill. Terminal products are DEF header tanks, day tanks, dispensing cabinet reservoirs, and service-engine compartment reservoirs with volumes from 10 L to 2,000 L. The red pigment does not contribute to the leachate load when fully encapsulated, but the same lot must still be tested for batch-to-batch extractable consistency because the pigment dispersion quality can affect the surface-to-volume ratio of exposed organic material.
Across marine navigation buoy and fender programmes, the red pigmentation of Icorene 1761 RED 4308 is used for high-contrast daytime marking without secondary coating, eliminating the paint adhesion step that normally introduces solvents and edge-peeling failure after repeated hull contact. The relevant material compliance framework is ASTM G154-16 accelerated weathering and ASTM D256-23 notched Izod impact after weathering, while buoy colour is matched to IALA surface colour recommendations rather than to a generic RAL reference. In this route, the powder is dry-blended with 0.20–0.40 wt% of a high-molecular-weight HALS and 0.10–0.20 wt% of a UV absorber whenever the base grade is not already marine-stabilised; the blend is tumbled for 12–15 min at 28 rpm in a ribbonless drum blender to prevent striation of low-density additives. Rock-and-roll moulding of a cylindrical buoy body with 900 mm major diameter and 10 mm nominal wall uses an oven setpoint of 260–275 °C, a PIAT of 190–200 °C, and a first-stage forced-air cooling rate of 4–6 °C/min down to 90 °C. Water-spray cooling is avoided because non-uniform heat extraction on the curved upper crown produces flat spots and dimensional warpage above 2.0 mm/m. Terminal products are navigation buoy shells, fender cores, flotation collars, and net-marking floats; many of these are filled with closed-cell polyurethane foam at 8–12 % of cavity volume after the shell reaches ambient temperature. Published data for this specific red-pigmented grade in saltwater and UV co-exposure beyond 5,000 h is limited; material substitution should be confirmed with retained impact and modulus data from the actual marine exposure zone.
Under non-food bulk solids service conditions, industrial hoppers and chute liners rotomoulded from Icorene 1761 RED 4308 must balance flexural stiffness, abrasion resistance, and intermittent impact from lump solids without contaminating the handled product. The mechanical qualification suite is ASTM D790-17 and ISO 178:2019 for flexural modulus, ASTM D638-14 for tensile yield, and ASTM D256-23 for Izod impact. Because most of these applications are non-food, the formulation can include 0.05–0.10 wt% of an internal slip additive such as erucamide or oleamide only where powder or dust build-up is a verified flow problem; the additive is introduced as a pre-compounded masterbatch rather than as a dry-blended wax because dry-blended amides can segregate toward the inner surface during oven rotation and create a greasy film on wear surfaces. Processing on a clamshell machine with cast aluminium tooling and heating zones controlled to ±5 °C uses an oven setpoint of 270–285 °C and an internal air temperature of 190–198 °C. Cooling is forced air until the part reaches 80 °C, followed by water mist at 30–35 °C for 8–10 min to lock in dimensions. Terminal products include bulk storage hoppers, vibratory bowl liners, chute transitions, weigh-hopper liners, and skip bucket liners with service volumes from 50 L to 4,000 L. The red-pigmented variant is not qualified for direct food-contact use unless a specific FDA 21 CFR 177.1520 exemption letter is provided by the supplier for the exact colorant package.
As a UN-rated packaging substrate, Icorene 1761 RED 4308 must pass stack, drop, and hydraulic pressure tests before chemical compatibility is considered. Under 49 CFR 178.603 and the parallel ADR 6.1.5 provisions, rotomoulded inner receptacles are subjected to drop testing at -18 °C after conditioning, stack testing at 40 °C for 28 days, and hydraulic pressure testing for liquid packagings depending on vapour pressure and filling degree. In this route, regrind from the same pre-coloured grade is permitted at 15–25 wt% only when produced from clean trim of the same lot and ground to a particle size within 250–600 µm; cross-lot regrind is not automatically acceptable because UN performance tests are formulation-specific and the red pigment package affects wall thickness distribution through melt-flow shift. The process uses a single-arm shuttle machine with two identical aluminium moulds and individual internal air temperature probes; the target PIAT is 190–205 °C, with oven dwell adjusted in 2 min increments until the wall at the top shoulder and bottom corner differs by no more than 0.5 mm. Terminal products are UN-rated jerrycans, inner receptacles for combination packaging, and open-head solids drums with volumes between 20 L and 220 L. Because the red pigment package contributes to the specific gravity of the final wall, a formulation-density check under ASTM D1505-18 is required for each new production batch before declaring equivalency to a natural grade.
Competitive LyondellBasell Icorene 1761 RED 4308 Polyethylene, Linear Low Density, Metallocene prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
LyondellBasell Icorene 1761 RED 4308 is a precompounded rotational molding powder based on a metallocene linear low density polyethylene. The designation separates the Icorene 1761 base resin from the RED 4308 colorant system. Published typical data for the unpigmented Icorene 1761 base resin list a nominal density of 0.938 g/cm³ when tested in accordance with ISO 1183-1:2019 and a melt mass-flow rate of 5.0 g/10 min at 190 °C under 2.16 kg load using ISO 1133-1:2022. The metallocene catalyst system produces a narrower molecular weight distribution and more uniform short-chain branching than conventional Ziegler-Natta LLDPE, which shifts the balance of sintering, low-temperature impact, and environmental stress crack resistance. The RED 4308 pigment package is incorporated by melt compounding rather than dry blending, eliminating a separate colorant let-down step and reducing batch-to-batch color variability on carousel or shuttle rotational molding lines.
| Property | Test method | Typical value | Unit |
|---|---|---|---|
| Density | ISO 1183-1:2019 | 0.938 | g/cm³ |
| Melt mass-flow rate | ISO 1133-1:2022, 190 °C/2.16 kg | 5.0 | g/10 min |
| Tensile stress at yield | ISO 527-2:2012, type 1A, 50 mm/min | 17 | MPa |
| Tensile strain at break | ISO 527-2:2012 | 750 | % |
| Flexural modulus | ISO 178:2019 | 550 | MPa |
| Charpy notched impact at −40 °C | ISO 179-1:2010 | 9 | kJ/m² |
| Environmental stress crack resistance, F50, 10% Igepal CO-630, 50 °C | ASTM D1693-15b | >1000 | h |
| Vicat softening temperature, A50 | ISO 306:2022 | 114 | °C |
| Melting peak temperature | ISO 11357-3:2018 | 126 | °C |
The values above are manufacturer-reported typical values for the unpigmented Icorene 1761 base resin and are not release criteria for the pigmented RED 4308 configuration. Published data for this specific pigmented variant are limited; therefore, any process-capability limit or acceptance criterion should be verified against the certificate of analysis supplied with each production batch.
In rotationally molded parts, the densification behavior of metallocene LLDPE is controlled by the peak internal air temperature and the residence time above the melting peak. For Icorene 1761, the melting peak is approximately 126 °C under ISO 11357-3:2018, but full densification requires the mold internal air to reach between 200 °C and 230 °C. The lower boundary is dictated by incomplete particle coalescence; the upper boundary is dictated by thermo-oxidative chain scission and potential color shift of the red 4308 pigment. On production-scale shuttle and carousel machines, a frequently observed failure mode is pinhole formation at wall thickness transitions, particularly at rib roots and flange radii, where local cooling rates are higher. Increasing the peak internal air temperature in 5–10 °C increments is the typical corrective action, but this must be balanced against increased cycle time and molded-in stress.
Forced-air convection ovens with air velocities in the range of 3–7 m/s are used to heat the mold. Because polyethylene powder is a poor thermal conductor, the heating segment is not uniform through the part cross-section. The controlling variable is not the oven set point but the internal mold air temperature, which is measured with a thermocouple inserted through a vent. A rotation ratio of 4:1 on biaxial machines is commonly employed; ratios of 2:1 to 6:1 may be required for asymmetric mold geometry to prevent wall thinning at flanges. The powder particle size distribution for rotational molding grades is typically specified with a maximum particle size near 35 mesh (500 μm) and a fines fraction below 10% by mass. Coarse particles can leave pinholes; excessive fines can create melt-starved areas and reduce bulk flow in the mold cavity. Moisture adsorption above 0.05% by mass should be avoided by storing the powder in sealed containers at relative humidity below 70%. If surface moisture is present, venting during the early heating stage is required to prevent steam porosity. The grade should not be processed above 260 °C internal air temperature for prolonged periods because chain scission and pigment degradation may proceed simultaneously.
The red 4308 colorant system is typically incorporated into the base resin on a co-rotating twin-screw extruder with an L/D ratio of 40:1 to 44:1, using distributive mixing elements rather than high-shear kneading blocks to minimize localized temperature rise. This compounding step affects the final powder characteristics because the pigmented compound is subsequently pulverized. Variations in pigment dispersion quality can shift low-temperature impact and environmental stress crack resistance; hence, the certificate of analysis should include melt mass-flow rate, density, and colorimetric data for each pigmented batch. A colorimeter shift of more than 1.0 ΔE from the approved standard can indicate insufficient pigment dispersion or concentrate metering drift during compounding.
Mechanical benchmarks for the unpigmented Icorene 1761 base resin are listed in the table above. Tensile yield stress at 50 mm/min according to ISO 527-2:2012 is approximately 17 MPa, and tensile strain at break is approximately 750%. The flexural modulus is approximately 550 MPa under ISO 178:2019, placing the grade in the medium-stiffness class for rotationally molded polyethylene. Notched Charpy impact at −40 °C is approximately 9 kJ/m² under ISO 179-1:2010; red pigments can reduce low-temperature impact by 10–20% depending on dispersion quality and particle size distribution. Environmental stress crack resistance measured under ASTM D1693-15b in 10% Igepal CO-630 at 50 °C exceeds 1000 h for the base resin. This is a significant differentiation from conventional Ziegler-Natta LLDPE rotational molding grades of similar melt index, which often fail below 500 h under the same conditions. The Vicat softening temperature is approximately 114 °C under ISO 306:2022 A50 loading, and the melting peak is 126 °C under ISO 11357-3:2018.
The metallocene architecture narrows the molecular weight distribution and reduces the high-molecular-weight tail that dominates melt elasticity. In rotational molding, this lowers low-shear viscosity and shortens the sintering time at a given oven temperature compared with conventional Ziegler-Natta LLDPE of equivalent density and melt index. The penalty is lower melt strength, which can produce sagging on vertical mold walls if the peak internal air temperature is excessive. Operators sometimes reduce peak internal air temperature by 5–10 °C relative to conventional LLDPE. Compared with autoclave LDPE, the Icorene 1761 base resin has higher stiffness and better ESCR but lower melt strength and less clarity. Compared with Ziegler-Natta LLDPE, the metallocene grade exhibits improved dart impact at low temperature and more consistent comonomer distribution, reducing warpage at weld lines. The red 4308 pigment system is not a simple dry blend; its presence modifies the rheological and thermal profile and must be accounted for when transferring a process from natural, black, or masterbatch-colored materials.
Single-site catalysis also reduces the concentration of low-molecular-weight and oligomeric species. This is relevant for extraction and organoleptic performance. Total hexane extractables of the unpigmented base resin are typically below 2.0% by mass under the extraction procedure referenced in FDA 21 CFR 177.1520. Conventional autoclave LDPE grades may exceed 3.0% hexane extractables under comparable conditions. The lower extractables profile supports applications in food-contact and pharmaceutical packaging only when the final pigmented article is approved through the required migration testing.
Precolored grades eliminate the separate addition of a color concentrate, but the processor loses the ability to adjust color loading without dry blending. Red organic pigments may have different infrared absorption characteristics than carbon black or titanium dioxide, so the heating cycle used for black or natural parts cannot be transferred directly. In outdoor applications, the red 4308 colorant concentration is not necessarily optimized for ultraviolet retention; weathering performance must be verified according to ISO 4892-2:2013 or ASTM G154 on the finished part. Pigment migration in polymer matrices is also a consideration when the molded article contacts fatty food simulants or hydrocarbons. Migration kinetics of the red colorant system must be evaluated under EU 10/2011 or FDA 21 CFR 177.1520; base resin compliance does not automatically extend to the pigmented article.
Typical application contexts for Icorene 1761 RED 4308 include rotationally molded chemical storage tanks, agricultural containers, marine buoys, and outdoor equipment where red color coding serves safety or brand identification. The grade is not recommended for continuous immersion in strong mineral acids or oxidizing media above 50 °C because polyethylene undergoes oxidative embrittlement and stress cracking at elevated service temperatures. For fuel-containing applications, permeation resistance must be evaluated under ASTM D814 or equivalent because LLDPE is not a barrier resin. In potable water contact, extraction testing under NSF/ANSI 61 or equivalent local regulation is required on the finished article; compliance of the base resin alone is insufficient to certify a pigmented part.
| Regulation / standard | Clause / test designation | Applicability boundary |
|---|---|---|
| FDA 21 CFR | 177.1520(c) 3.1a/3.2a | Unpigmented base resin only; RED 4308 pigment package must be separately evaluated for final article food-contact status |
| EU Plastics Regulation | EU 10/2011, Annex I | Overall migration limit 10 mg/dm²; specific migration limits for pigment components must be tested on finished article |
| REACH SVHC | Regulation (EC) No 1907/2006, Article 33 | No SVHC above 0.1% w/w declared in base resin; RED 4308 concentrate requires supplier confirmation |
| RoHS | Directive 2011/65/EU, Annex II | Cadmium 100 ppm; lead, mercury, hexavalent chromium, PBB, PBDE each 1000 ppm at homogeneous material level |
For food-contact evaluation, the uncolored base resin may be described by FDA 21 CFR 177.1520 olefin polymer provisions when the density and melt index remain within the specified limits. The red 4308 pigment package requires separate migration testing because organic pigments and their dispersants can contribute to overall migration. Under EU 10/2011, the overall migration limit is 10 mg/dm² of contact area for food contact articles, and specific migration limits apply to individual pigments and processing aids. If the article is exported to jurisdictions requiring positive list approval for colorants, the colorant components must be listed in the applicable positive list. No statement should be made that the red 4308 grade is FDA-compliant without a written certificate from the pigment supplier and a migration test on the final molded article.