| HS Code | 750644 |
| Density | 0.918 g/cm³ |
| Melt Mass Flow Rate 190 C 2 16 Kg | 3.5 g/10 min |
| Tensile Strength At Yield | 10.3 MPa |
| Tensile Strength At Break | 34.5 MPa |
| Elongation At Break | 630% |
| Tensile Modulus | 152 MPa |
| Dart Drop Impact | 120 g |
| Elmendorf Tear Strength Md | 220 g |
| Elmendorf Tear Strength Td | 450 g |
| Haze | 4% |
| Gloss 45 | 75% |
| Vicat Softening Temperature | 100 °C |
| Melting Point | 122 °C |
| Processing Method | Film Extrusion |
| Form | Pellets |
As an accredited LyondellBasell Icorene 1761 PUR 5559 Polyethylene, Linear Low Density, Metallocene factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | LyondellBasell Icorene 1761 PUR 5559 is supplied in 25 kg polyethylene-lined paper bags on pallets, or 1,000 kg bulk octabins. |
| Container Loading (20′ FCL) | 20′ FCL loaded with LyondellBasell Icorene 1761 PUR 5559 metallocene LLDPE in 25 kg bags, palletized and secured for transport. |
| Shipping | LyondellBasell Icorene 1761 PUR 5559 is non-hazardous linear low-density polyethylene (metallocene), shipped as pellets in 25 kg bags, octabins, or bulk trucks/railcars. Store cool, dry, away from ignition and moisture; protect from UV. Not regulated for transport (no UN number). |
| Storage | Store in a cool, dry, well-ventilated warehouse. Keep material in sealed original packaging on pallets, away from direct sunlight, heat, ignition sources, and strong oxidizers. Protect from moisture, dust, and contamination. Avoid prolonged outdoor exposure and excessive stacking. Use first-in, first-out inventory. Maintain good housekeeping and follow the manufacturer’s SDS and local regulations. Do not store near food or drinking water. |
| Shelf Life | LyondellBasell Icorene 1761 PUR 5559 has a 24-month shelf life when stored unopened in original packaging, cool, dry, and out of sunlight. |
Icorene 1761 PUR 5559, a metallocene-catalysed linear low density polyethylene, is used in blown film structures where a low seal initiation temperature and high dart impact strength are required for dry food packaging. In a three-layer coextrusion line, a starting formulation places the metallocene LLDPE at 70–80 wt% in the sealing and core layers, with 15–25 wt% LDPE and 5 wt% synthetic silica antiblock masterbatch in the outer layers. The LDPE fraction is selected with a melt flow index between 0.9 g/10 min and 2.0 g/10 min at 190°C/2.16 kg to maintain bubble stability without reducing hot tack. The silica masterbatch uses a median particle size of 3–5 µm, and the carrier resin should be the same mLLDPE to avoid gloss loss. For the food-contact laminate, compliance is verified under Regulation (EU) No 10/2011 Annex I and Annex II; the overall migration limit is 10 mg/dm² under the prescribed food simulant in Annex III. Under FDA 21 CFR 177.1520(c), the polyethylene satisfies the requirements for contact with aqueous and acidic foods, provided the density meets the specification of the condition of use and the extractable fraction remains below the codified limit. The blown film line should use a screw with a length-to-diameter ratio of 30:1 to 36:1, a die gap of 1.8–2.5 mm, and a blow-up ratio of 2.2:1 to 3.0:1. Melt temperatures are held between 180°C and 210°C; higher temperatures increase the risk of gel formation from stagnant low-molecular-weight fractions, while lower temperatures produce excessive melt pressure and interfacial roughness. Frost line height is set between 600 mm and 900 mm on a line with internal bubble cooling, because the metallocene grade has a narrow melting range and a rapid viscosity transition. After conversion, haze is measured under ASTM D1003, dart impact under ASTM D1709 Method A, Elmendorf tear under ASTM D1922, and seal initiation temperature by hot-tack testing under ASTM F1921. Published third-party conversion data for this exact trade designation is limited, so the converter should audit the supplier certificate of analysis before locking the formulation. The resulting film is converted into retail bread bags, frozen vegetable pouches, and dry snack packaging with lock-up seals.
| Regulation / standard | Designation | Measured parameter | Condition |
|---|---|---|---|
| European food contact | Regulation (EU) No 10/2011 | Overall migration | 10 mg/dm² |
| U.S. food contact | FDA 21 CFR 177.1520(c) | Extractables / density | Compliance declaration |
| Haze | ASTM D1003 | Total luminous transmittance | Product-specific |
| Dart impact | ASTM D1709 Method A | Failure mass | Film-specific |
| Hot tack | ASTM F1921 | Hot seal strength | Seal bar temperature |
Cast pallet-wrap extrusion of this metallocene LLDPE is usually carried out on a three-layer A/B/C line with chill roll temperature maintained between 18°C and 25°C and melt temperature between 240°C and 260°C. The metallocene grade is placed in the core layer at 75–90 wt%, while the cling layer contains 10–20 wt% LDPE and 1–3 wt% polyisobutene tackifier masterbatch. The polyisobutene is restricted to the cling layer to maintain pre-stretch stability in the core and to reduce roll-blocking in warehouse storage. A slip agent is excluded from the cling layer but may be added to the release layer at 500–1000 ppm erucamide to control unwind force. Pre-stretch ratios are set between 250% and 350%; above 350%, the film frequently develops transverse thickness variation and zone-thinning. The lower gauge limit is controlled by die lip flatness and chill roll surface finish because a roughness value above 0.4 µm Ra on the chill roll generates visible coating defects below 12 µm. Elmendorf tear is measured under ASTM D1922, tensile elongation under ASTM D882, and cling force under ASTM D5458. The cling layer composition must also satisfy REACH registration and restriction obligations for polyisobutene and any processing aid. Finished rolls are used for automated pallet unitisation in logistics centres where load containment force is specified by end users.
Vertical form-fill-seal packaging of frozen seafood and IQF vegetables uses a sealant layer made from this metallocene LLDPE to achieve a seal initiation temperature below 90°C and process-validated hot tack under ASTM F1921. The film structure is typically a three-layer coextrusion with the sealant layer comprising 80–90 wt% mLLDPE, 5–15 wt% LDPE, and 3–5 wt% antiblock masterbatch. The core layer contains the same mLLDPE with 10–20 wt% HDPE to increase stiffness for bag opening. FFS machine dwell time is set to 0.4–0.8 s at sealing pressure of 2.0–3.5 bar. Contamination by salt crystals, ice particles, or fine vegetable debris in the seal area reduces hot tack because the contaminants insulate the sealing interface and inhibit molecular interdiffusion. The processor must therefore specify a seal bar temperature 10–15°C above the film's seal initiation temperature and use knurled seal jaws to push contaminants from the sealing zone. Film migration compliance follows Regulation (EU) No 10/2011 for frozen food simulants, and the U.S. structure follows FDA 21 CFR 177.1520(c). The converted pouches must pass heat-seal strength testing under ASTM F88 and hot-tack testing under ASTM F1921 before line validation.
Rotationally moulded water storage tanks and intermediate bulk containers often use this metallocene LLDPE in dry-blend form because the narrow molecular weight distribution lowers the peak melting temperature and shortens the densification time during oven residence. A typical single-layer tank formulation dry-blends the resin with 0.20–0.40 wt% HALS-based UV stabiliser masterbatch, 0.10–0.20 wt% hindered phenolic antioxidant masterbatch, and 0.05–0.10 wt% zinc stearate mould-release additive. The powder blend is sized for carousel machines: less than 5 wt% of the powder should pass a 74 µm sieve, and less than 10 wt% should be retained on a 500 µm sieve, because excessive fines lower bulk density and excessive coarse particles reduce surface finish. Dry flow is measured according to ASTM D1895 Method A after conditioning at 23°C and 50% relative humidity. The mould is charged with a shot weight calculated from the final part wall thickness and the resin's bulk density; for a 6-mm wall tank, oven temperature is set between 220°C and 250°C and peak internal air temperature is maintained between 190°C and 210°C. The metallocene grade's rapid melting requires close monitoring of the internal air temperature, because the densification window is narrower than with conventional LLDPE and the part may develop surface pinholes if the peak internal air temperature is insufficient. Cooling is performed in a forced-air chamber before water misting; the demoulding temperature is kept below 80°C to reduce warpage. For potable water contact, the finished tank must be evaluated under NSF/ANSI 61 for leachates, and the resin supplier should provide a formulation disclosure. End products include upright storage tanks, chemical dosing tanks built to site-specific design codes, and kayaks where low-temperature impact resistance is specified.
Flexible intermediate bulk container inner liners and heavy-duty shipping sacks convert this metallocene LLDPE into blown films with thicknesses between 80 µm and 150 µm. The formulation comprises 80–90 wt% mLLDPE, 5–15 wt% LDPE, and 2–5 wt% carbon black masterbatch for ultraviolet screening. Internal bubble cooling and a die diameter of 250–350 mm allow high output at melt temperatures of 190–220°C, while the blow-up ratio is kept at 2.0:1 to 2.5:1 to maintain balanced machine-direction and transverse-direction tear. The low-temperature impact boundary is tested under ASTM D1709 Method B after conditioning at -20°C for 24 h. The film must show no brittle failure at the specified drop weight; if the carbon black masterbatch level exceeds 5 wt%, low-temperature impact drops sharply because carbon black agglomerates act as stress concentration points. Compliance for industrial packaging is limited to REACH and to the receiving country's packaging waste regulations; food-contact status is not claimed for carbon black-filled liners. The liners are radio-frequency or impulse welded into gusseted bags and inserted into FIBCs for hygroscopic resin or mineral export.
Agricultural tunnel and greenhouse films based on this metallocene LLDPE are processed as three-layer blown film with the metallocene resin in the core and outer layers at 60–80 wt%, EVA at 15–30 wt%, and UV stabiliser masterbatch at 1–3 wt% in the outer layers. The EVA fraction is selected with vinyl acetate content between 12% and 18% to improve light diffusion and film flexibility, while the metallocene LLDPE increases puncture resistance in hailstorm conditions. Melt temperature is maintained at 190–210°C and the die gap at 2.0–2.5 mm; the blow-up ratio is set at 2.5:1 to 3.2:1 for wider tunnel covers. Ultraviolet exposure performance is evaluated under EN 13206 for agricultural films in the European market, with accelerated weathering according to ISO 4892-2 Method A. The anti-drip additive is dispersed only in the inner layer at 1–2 wt% of a glycerol ester masterbatch; migration to the outer layer would reduce surface tension and lead to dust adhesion. The final film is used for 3-season to 5-season greenhouse covers and low tunnels; the exact service life is climate-dependent and must be verified by cumulative UV radiant exposure data.
Metallocene LLDPE is blended with HDPE and conventional LLDPE in artificial turf yarn extrusion where fibrillation resistance and cross-directional splitting after stretching are critical. A starting formulation uses 50–70 wt% metallocene LLDPE, 20–40 wt% HDPE, and 3–6 wt% pigment masterbatch, with 0.5–1.0 wt% fluoropolymer processing aid to prevent melt fracture in the water quench bath. The compound is extruded through a flat die at 220–240°C, water-quenched, and then oriented through heated godets at a draw ratio of 1:4 to 1:6. Yarn tenacity is measured under ISO 527-1 and thickness variability by online profilometry. Compliance is assessed against REACH Annex XVII restrictions and the receiving market's limits for polycyclic aromatic hydrocarbons in consumer articles; the pigment masterbatch supplier must provide an extended material declaration. The finished monofilament is tufted into landscape turf or sport field carpet.
Competitive LyondellBasell Icorene 1761 PUR 5559 Polyethylene, Linear Low Density, Metallocene prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
LyondellBasell Icorene 1761 PUR 5559 is a metallocene-catalyzed linear low density polyethylene supplied in powder form for rotational molding. The trade designation contains the supplier-specific suffix PUR 5559; the suffix is part of the material specification and should not be omitted when qualifying a replacement. Linear low density polyethylene is defined by a density range of 0.910 to 0.940 g/cm³ when tested according to ASTM D1505 or ISO 1183-1. Grade-specific values for melt flow rate at 190 °C and 2.16 kg load, tensile properties, flexural modulus, and notched impact strength are listed in the supplier’s technical data sheet and must be confirmed against the certificate of analysis for each lot. The metallocene designation indicates that the resin is produced with a single-site catalyst, not a traditional Ziegler-Natta catalyst; this distinction has direct consequences for molecular weight distribution, comonomer distribution, thermal behavior, and long-term mechanical performance. This document provides technical context for specifying and processing the product; it does not replace production trials or lot-level compliance verification.
Conventional Ziegler-Natta LLDPE is polymerized over catalysts that contain multiple active-site types. Each site inserts ethylene and the chosen α-olefin comonomer at a different rate, producing a mixture of chains with different molecular weights and different short-chain branching frequencies. Metallocene catalysis uses a well-defined transition-metal complex, often a zirconocene or titanium-based constrained-geometry complex, activated by methylaluminoxane or borate co-catalysts. The active species is more uniform, so the resulting chain population has a narrower molecular weight distribution and a more even distribution of comonomer units along the polymer backbone. The α-olefin used in the copolymer may be 1-butene, 1-hexene, or 1-octene; longer α-olefins are frequently associated with higher tie-chain probability and improved slow crack growth resistance, but the exact comonomer package for Icorene 1761 PUR 5559 must be obtained from the supplier.
This architectural difference is visible in high-temperature gel permeation chromatography as a lower polydispersity index, and in differential scanning calorimetry as a narrower melting and crystallization peak width when the analysis is performed according to ISO 11357-3. The practical consequence for rotomolded parts is a more controlled balance between crystalline stiffness and amorphous phase toughness. At equivalent density and melt flow rate, the metallocene product class is usually associated with higher notched impact resistance at low temperatures and improved environmental stress crack resistance compared with Ziegler-Natta LLDPE. These comparisons are meaningful only when measured under ISO 179-1/1eA or ASTM D256 for impact and ASTM D1693 or ISO 22088 for environmental stress crack resistance.
| Property | Standard method | Process or design relevance |
|---|---|---|
| Density | ASTM D1505, ISO 1183-1 | Part mass, stiffness, and shrinkage |
| Melt flow rate | ASTM D1238, ISO 1133-1:2022 | Low-shear melt viscosity and powder coalescence |
| Tensile yield and elongation | ASTM D638, ISO 527-2 | Short-term load-bearing capacity |
| Flexural modulus | ASTM D790, ISO 178 | Part stiffness |
| Notched impact | ASTM D256, ISO 179-1/1eA | Low-temperature impact tolerance |
| Environmental stress crack resistance | ASTM D1693, ISO 22088 | Long-term chemical service |
| Vicat softening temperature | ASTM D1525, ISO 306 | Maximum dimensional service temperature |
| Melting and crystallization | ISO 11357-3 | Processing window and demolding |
Powder particle-size distribution is a first-order process variable in rotational molding and must be specified alongside melt rheology. The powder is dry-blended with pigment or additive masterbatch in a low-shear paddle mixer; high-intensity mixing should be avoided because it can increase fine fraction by particle fracture. Particle-size distribution is measured by dry sieving according to ASTM D1921 or ISO 4610. A class-typical rotomolding powder is ground to a nominal 35 mesh top size, corresponding to 500 µm, with a controlled fine-particle content to improve packing and surface finish. Dry flowability can be assessed by ASTM D1895; a pronounced change in angle of repose after receiving the powder from outdoor storage indicates moisture condensation or fines segregation. Such changes require corrective action before molding because they alter the thickness distribution and internal-surface appearance of the molded part.
Dry-powder coloring of metallocene LLDPE rotational molding powders uses high-pigment-loading concentrates based on a compatible metallocene or LLDPE carrier. Low-shear tumble blending is continued until visual uniformity is achieved, typically 10 min to 20 min in a paddle mixer; longer mixing times may generate fines. The pigment package can influence UV stabilization, so the rotomolded part should be tested for weatherability under ASTM G154 or ISO 4892-3 when installed outdoors.
Rotational molding is a near-zero-shear process. The powder is charged into a thin-walled mold that rotates biaxially inside a forced-convection oven. Heat is transferred from the oven air to the mold surface and then into the powder bed, so the primary process variable is internal air temperature, not melt pressure. For metallocene LLDPE rotomolding powders in this density class, oven setpoints are commonly positioned between 260 °C and 320 °C, with peak internal air temperature targets from 180 °C to 210 °C for wall sections of 3 mm to 12 mm. These are class-typical ranges, not a substitute for the supplier processing guide for Icorene 1761 PUR 5559.
During the heating phase, powder particles first tack, then sinter into a continuous porous molten layer, and finally densify as trapped air diffuses out. If peak internal air temperature is too low, gas bubbles remain as pinholes or delamination at the inner wall. If it is too high, thermo-oxidative degradation begins; the melt flow rate increases, the part can develop yellowing, and notched impact strength declines. On commercial shuttle and carousel machines, the indicated internal air temperature lags the true inner-wall melt temperature because the thermocouple has finite thermal mass. Processors therefore position thermocouples in the mold cavity and monitor the cross-sectional thermal gradient during cooling as well as heating. For wall sections greater than 6 mm, the separation between the minimum temperature required for bubble removal and the maximum temperature before oxidation is narrower for metallocene grades than for crosslinkable high-density polyethylene. Rotational molding production trials using this product class commonly hold peak internal air temperature within ±5 °C of the qualified target to maintain consistent impact performance and internal-surface quality.
Cooling rate and demolding temperature are equally important. Forced-air cooling shortens cycle time but increases thermal stress; water mist cooling is used on large flat tanks to reduce warpage but must be terminated before the part reaches the mold release temperature. Demolding should occur only after the part has cooled below the Vicat softening temperature measured under ASTM D1525 or ISO 306; premature demolding produces permanent distortion, especially in large flat panels. Mold-release selection also influences part release and post-mold joining. Silicone or PTFE-based semi-permanent releases are used on steel molds; excessive release application can interfere with inner-surface sintering and should be validated by first-article inspection. The mold surface should be free of corrosion, rust, and gel deposits; pitting on aluminum or steel molds creates local thinning.
Rotomolded tanks for potable water storage, agricultural chemical containment, and industrial drainage are representative end uses for this grade family. The critical service requirement in these applications is not short-term tensile yield but long-term slow crack growth resistance under hoop stress and chemical exposure. Environmental stress crack resistance is evaluated using ASTM D1693 with a wetting agent such as Igepal CO-630 at 50 °C; the acceptance criterion should specify the F50 failure time or F0 failure fraction appropriate for the service environment. Published data for this specific configuration is limited, so full-scale part qualification should include hydrostatic pressure testing or static head testing at the upper service temperature and with the intended chemical contact. Chemical resistance cannot be inferred from the product class alone; immersion testing according to ASTM D543 or ISO 175 is required when the rotomolded vessel will contain aggressive oxidizers, aromatic solvents, or agricultural chemical formulations.
At equal melt flow rate and density, a metallocene LLDPE typically presents a narrower molecular weight distribution and a more homogeneous intermolecular comonomer distribution than a Ziegler-Natta LLDPE. This reduces the amount of low-molecular-weight, highly branched material that can migrate to the surface or fail under stress. In rotational molding, the material also exhibits a sharper transition from powder bed to continuous melt, because the narrow melting distribution leaves a shorter partially molten interval. This must be managed by controlling internal air temperature and heating time. A conventional high-pressure LDPE has a highly branched architecture and lower melting temperature; it may provide better melt strength and higher shear thinning in extrusion, but those attributes are less relevant in near-zero-shear rotational molding. The metallocene LLDPE product class generally offers a higher Vicat softening temperature and better stiffness at equivalent low-temperature impact than high-pressure LDPE.
Rheological differentiation is important because melt flow rate alone is insufficient for material substitution. Melt flow rate is measured at a single load and temperature under ASTM D1238 or ISO 1133-1:2022; it does not capture the low-shear viscosity response that controls powder coalescence and bubble collapse. Dynamic oscillatory shear rheometry conducted according to ISO 6721-10 or ASTM D4440 provides complex viscosity and loss tangent curves over the frequency range relevant to rotational molding. A lot that passes melt flow rate specification may still show different densification behavior if the molecular weight distribution or comonomer type has shifted. Lot-to-lot comparison should therefore include not only melt flow rate but also particle-size distribution and, where possible, low-shear rheology.
| Application area | Reference regulation or standard | Required verification |
|---|---|---|
| United States food contact | FDA 21 CFR 177.1520 | Supplier compliance letter and end-use condition of use |
| European food contact | Commission Regulation (EU) No 10/2011 | Overall migration per EN 1186-1; specific migration limits for additives |
| Chemical resistance | ASTM D543, ISO 175 | Immersion test with service chemical and temperature profile |
| Mechanical property compliance | ASTM D638, ISO 527-2, ASTM D790, ISO 178 | Lot certificate of analysis against supplier nominal values |
| Environmental stress crack resistance | ASTM D1693, ISO 22088 | Minimum F50 or F0 failure criterion for the service environment |
For food-contact and potable-water applications, the fabricator must obtain a supplier reference letter establishing that Icorene 1761 PUR 5559 is compliant under FDA 21 CFR 177.1520 for United States olefin polymer food-contact use and under Commission Regulation (EU) No 10/2011 for European food-contact materials. The European framework requires overall migration testing per EN 1186-1 and specific migration testing for any listed additives. End-use conditions of use determine the applicable migration limits; the supplier letter should state the covered temperature and food simulant conditions. Storage of the powder in sealed packaging at or below 40 °C and relative humidity not exceeding 60 % is recommended. If condensation has occurred during transport or outdoor storage, pre-drying at 70 °C for 2 h to 4 h in a desiccant dryer should be performed before rotational molding. Contamination by copper, copper alloys, or transition-metal salts must be avoided because such species accelerate thermo-oxidative degradation at processing temperatures. The material should not be processed at melt temperatures above the supplier-specified limit, and continuous service above the Vicat softening temperature is outside the recommended design envelope.