| HS Code | 374915 |
| Color | Gray |
| Density | 0.918 g/cm³ |
| Melt Index | 1.0 g/10 min |
| Melting Point | 118 °C |
| Vicat Softening Temperature | 100 °C |
| Tensile Strength At Yield | 10.3 MPa |
| Tensile Strength At Break | 40.0 MPa |
| Elongation At Break | 600% |
| Flexural Modulus | 200 MPa |
| Dart Drop Impact | 200 g |
| Elmendorf Tear Strength Md | 200 g/mil |
| Elmendorf Tear Strength Td | 400 g/mil |
| Haze | 10% |
| Gloss | 60% |
As an accredited LyondellBasell Icorene 1761 GRY 7736 Polyethylene, Linear Low Density, Metallocene factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | LyondellBasell Icorene 1761 GRY 7736 metallocene linear low density polyethylene is supplied in 25 kg bags, typically on pallets. |
| Container Loading (20′ FCL) | 20′ FCL loaded with LyondellBasell Icorene 1761 GRY 7736 metallocene linear low-density polyethylene, 25 kg bags, palletized, shrink-wrapped, and secured. |
| Shipping | LyondellBasell Icorene 1761 GRY 7736 is shipped as non-hazardous metallocene linear low-density polyethylene resin, usually in 25 kg bags or bulk containers on pallets. It is not regulated for transport; no UN number, hazard class, placards, or special documentation required. Keep dry, cool, and clean. Avoid excessive heat and moisture. |
| Storage | Store LyondellBasell Icorene 1761 GRY 7736 Polyethylene, Linear Low Density, Metallocene in a cool, dry, well-ventilated area away from direct sunlight, heat, sparks, and open flames. Keep original bags or containers sealed to prevent moisture, dust, and contamination. Avoid strong oxidizers. Use first-in, first-out rotation, maintain clean dry conditions, and follow the manufacturer’s SDS and local regulations. |
| Shelf Life | Shelf life is typically 24 months when stored in original unopened packaging, protected from heat, moisture, and direct sunlight. |
LyondellBasell Icorene 1761 GRY 7736 is supplied as a pre-grey pigmented metallocene linear-low-density polyethylene rotational molding powder. In above-ground stationary chemical and hydrocarbon containment systems, the resin is selected for low-temperature impact and environmental stress-crack resistance requirements associated with UN 1H1/Y1.5/250 single-pack intermediate bulk container qualification and EN 13575:2011 hydrostatic tests for static thermoplastic tanks. Molders processing this material for rectangular chemical bunds and vertical cylindrical tanks control the pulverized powder dry flow to 28–35 s/100 g under ASTM D1895-96 Method A and set oven temperatures between 280°C and 320°C, while peak internal air temperature measured by data-logging probes must remain between 190°C and 205°C. The pre-compounded grey colorant package eliminates separate pigment metering; where a conductive specification is required, 1.0–2.0 wt% conductive carbon black masterbatch is dry-blended for 15–20 min in a low-shear paddle mixer, and the addition increases peak internal air temperature by 8–12°C because of reduced powder bulk density. Cast-aluminum tooling with venting at 0.5–1.0 mm wall thickness is rotated at a 4:1 primary-to-secondary axis speed ratio, followed by forced-air cooling to a demolding temperature of 70°C or below; cooling rates above 5°C/min across the 60–90°C interval are avoided to preserve environmental stress-crack resistance. Representative terminal products include 5,000–30,000 L vertical storage tanks, dosing tanks, and secondary containment bunds designed for liquids with specific gravity up to 1.5.
In agricultural water storage and liquid fertilizer containment, the substitution of chromium-catalyzed LLDPE with Icorene 1761 GRY 7736 alters the cooling phase more than the heating phase. The narrower melting distribution requires a minimum peak internal air temperature of 195°C and a maximum of 215°C; below 195°C surface porosity increases, and above 215°C inner-wall oxidative yellowing can occur. The material is normally used at 100% as-supplied powder; for tropical installations, a maximum of 0.2–0.5 wt% hindered amine light stabilizer may be dry-blended, but the GRY 7736 pre-pigmentation already provides consistent grey UV shielding without additional masterbatch. Compliance for potable water contact is verified under NSF/ANSI/CAN 61 Section 5 in North America; in EU distribution, fertilizer tanks above 450 L used for transport are assessed as UN 1H1 packagings under ADR Chapter 6.1. The downstream process uses steel or cast-aluminum rotational molds with external release agents and a two-axis oven residency of 18–24 min; cooling is staged with 5 min ambient rotation followed by forced air at 0.8–1.2 m/s until internal air falls below 80°C. Typical finished parts include 5,000 L horizontal leg tanks, nurse tanks for fertilizer injection, and portable water bowsers.
| Application | Standard | Critical test | Acceptance boundary |
|---|---|---|---|
| Stationary chemical tank | EN 13575:2011 | Hydrostatic internal pressure at 1.5 times maximum working pressure | No leakage or visible deformation over 24 h |
| Agricultural water tank | NSF/ANSI/CAN 61 Section 5 | Extraction tests for metals and organic contaminants in cold water | Pass criteria per standard Annex B |
| Food handling bin | EU Regulation (EU) No 10/2011 | Overall migration in prescribed food simulants | ≤10 mg/dm² |
| Plastic fuel tank | UN ECE R34 Annex 5 | Impact, fire resistance, and permeability production audit | No rupture, no leakage, production approval |
In fish tub and insulated food handling bin production, the absence of a post-molding paint system is a compliance advantage because the food-contact surface is formed directly from the pigmented polyethylene layer. Icorene 1761 GRY 7736 is processed at 100% as-supplied powder for single-wall fish tubs; for insulated pallet boxes, the outer and inner shells are rotomolded separately and then bonded with a 2.5–5.0 cm polyurethane foam core at 30–40 kg/m³ density injected through sealed fill ports. The formulation must not exceed 1.0 wt% of any re-pigment masterbatch if a color change is specified for food branding; higher loadings can raise overall migration and complicate EU Regulation (EU) No 10/2011 overall migration compliance, which requires 10 mg/dm² maximum. In North America, the material falls under FDA 21 CFR 177.1520(c) 3.2a olefin polymer provisions; in China, GB 4806.7-2016 total migration and polymer-specific migration testing applies. Rotational molding for open-top fish tubs uses oven set-points of 270–300°C, peak internal air temperature of 190–205°C, and a cycle time of 12–18 min for wall thicknesses up to 6 mm. Terminal products include 100–600 L fish tubs, meat lugs, and insulated pallet boxes used in cold-chain distribution.
Rotational molders supplying play deck panels and outdoor seating in public parks process Icorene 1761 GRY 7736 in the same tooling used for HDPE but with a 10–15% lower oven temperature to prevent inner-wall polymer degradation at knit lines. The grey compound is used at 100% powder; where a different surface color is demanded, dry-blending a maximum of 1.5 wt% color masterbatch is accepted, but higher loadings of 2.0 wt% and above are avoided because large pigment particles nucleate shrinkage differences that cause warping in flat panels. Compliance under EN 71-3:2019+A1:2021 requires third-party migration testing for 19 elements; in practice, the pre-grey package is formulated to avoid lead, cadmium, and hexavalent chromium above detection limits, with specific migration limits per Table 2 of the standard. Mechanical safety evaluation follows EN 71-1:2014+A1:2018 for toys and ASTM F963-23 for the North American market. The downstream process uses cast-aluminum tools with oven set-points of 270–300°C, internal air temperature of 190–205°C, and total cycle times of 14–20 min; forced-air cooling must not exceed 1.5 m/s airflow on flat panels or differential shrinkage will produce visible bow. Terminal parts include climbing panels, slide hoods, spring rider bodies, and park benches.
| Nominal wall thickness | Oven set-point | Peak internal air temperature | Total oven residency | Cooling condition |
|---|---|---|---|---|
| 3–6 mm | 270–300°C | 190–205°C | 12–18 min | Forced air below 1.5 m/s, demolding 70°C |
| 6–10 mm | 290–310°C | 195–210°C | 16–24 min | Staged ambient/forced air, demolding 65°C |
| 10–15 mm | 310–320°C | 200–215°C | 25–30 min | Controlled cooling below 2°C/min, demolding 60°C |
Field data from rotational molders producing auxiliary diesel tanks for construction equipment show that Icorene 1761 GRY 7736 produces acceptable fuel resistance only when the inner wall is molded to a minimum thickness of 5.0 mm and the finished part is post-cured at 80°C for 2 h. The material is processed at 100% as-supplied grey powder; no fluorinated barrier additive is used for standard diesel tanks, but if electrostatic dissipation is specified, the rotomolder dry-blends 2.0–4.0 wt% conductive carbon black masterbatch, which raises required internal air temperature by 8–12°C and reduces powder flow through the mold during the first rotation phase. Compliance is verified under UN ECE R34 Annex 5 for plastic fuel tanks, while evaporative emission limits for nonroad equipment in the United States are addressed under 40 CFR Part 1060; published hydrocarbon permeation data for this specific configuration is limited, so production validation on each fuel tank geometry is required. The downstream process uses electroformed nickel or cast-aluminum tools, oven set-points of 280–310°C, peak internal air temperature of 200–210°C, and a controlled cooling rate below 2°C/min to minimize warpage at the filler neck and baffle bosses. Representative terminal products include 100–1,000 L diesel tanks for agricultural tractors, telehandlers, and generator sets.
Molders producing reusable pallet boxes, hopper liners, and drum handling pallets use Icorene 1761 GRY 7736 at 100% as-supplied powder to eliminate post-molding machining of corners and drain ports required by high-density polyethylene. The metallocene resin densifies at a lower peak internal air temperature of 185–195°C for wall sections below 6 mm; however, thick bin bases above 10 mm require oven set-points of 310–320°C and cycle times of 25–30 min to eliminate centerline porosity at the base-to-wall junction. Industrial pallet load performance is evaluated under ISO 8611-1:2021; in the EU supply chain, the molded article must meet REACH Regulation (EC) No 1907/2006 SVHC disclosure obligations. The downstream process uses sheet-steel tools with corner vents and a rotation speed ratio of 6:1 to fill deep ribs; cooling is forced air at 1.0–1.5 m/s followed by transfer to a flat cooling fixture before demolding at 60°C. Terminal products include heavy-duty pallet boxes, hopper liners for bulk solids, and drum handling pallets.
Competitive LyondellBasell Icorene 1761 GRY 7736 Polyethylene, Linear Low Density, Metallocene prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
LyondellBasell Icorene 1761 GRY 7736 is supplied as a metallocene-catalysed linear low-density polyethylene in a grey 7736 colour-matched system. The material belongs to the Icorene trade family, which designates single-site catalyst polyethylene grades rather than conventional Ziegler–Natta or high-pressure LDPE resins. The suffix GRY 7736 identifies a controlled grey pigmentation, not a natural pellet; therefore lot-specific colour strength, pigment loading, carrier resin composition, and stabiliser package must be verified on the certificate of analysis before conversion. The base polymer is typically characterised by a narrow molecular weight distribution and improved comonomer dispersion, which affect film toughness, sealing behaviour, and extrusion rheology.
Because published datasheet values for the GRY 7736-specific formulation may be limited, the following discussion separates base-resin behaviour from colour-related effects. Converters should obtain the manufacturer’s technical data sheet and compare the reported values against the actual lot certificate. Test methods commonly used for product release include ISO 1133-1:2022 for melt mass-flow rate, ISO 1183-1:2019 for density, ISO 527-2:2012 for tensile properties, ISO 178:2019 for flexural modulus, and ISO 306:2022 for Vicat softening temperature.
Conventional Ziegler–Natta LLDPE is produced with heterogeneous active sites that generate broad molecular weight and branching distributions. Metallocene catalysis replaces that distribution with a narrow molecular weight profile and more uniform comonomer placement. For Icorene 1761 GRY 7736, this architecture is expected to deliver higher dart impact strength, lower seal initiation temperature, and better optical clarity than a Ziegler–Natta LLDPE of similar density, although the grey pigmentation may reduce transparency. The trade-off is a reduction in shear thinning: at high extrusion rates the metallocene resin exhibits higher viscosity, which raises screw torque and die pressure. The material also generates lower melt tension than LDPE, so blown-film bubble stability can become limiting before throughput reaches LDPE levels.
The molecular weight distribution of metallocene LLDPE is typically narrower, with polydispersity indices in the range 2.0 to 2.5, compared with 3.5 to 4.5 for conventional LLDPE. This shift changes the shear-viscosity curve. The melt mass-flow rate at 190 °C and 2.16 kg load should be controlled to the manufacturer’s specification; if a target MFR of 1.0 g/10 min is assumed for a film grade, the viscosity at 100 s⁻¹ may be higher than a Ziegler–Natta LLDPE of equivalent MFR, causing greater die pressure. The tensile and impact advantages are linked to the more homogeneous comonomer distribution, which reduces the fraction of highly branched low-molecular-weight chains that lower toughness.
Extrusion lines for this product should be equipped with grooved feed sections, barrier screws, and screen packs rated for LLDPE pressures. On commercial cast-film and blown-film lines with L/D 30:1 screws, die pressures can be 15–30 % higher than LDPE at equivalent output. The die gap is typically held between 1.2 mm and 2.0 mm for blown film, with blow-up ratios of 2.0:1 to 3.0:1. Melt temperatures in the range 190 °C to 230 °C are common. If the screw is operated too hot, the narrow molecular weight distribution does not prevent degradation; it changes the failure signature toward gel formation and melt-flow shift. Start-up after a resin change should include purging with a low-MFR polyethylene or mechanical purging compound, because the grey 7736 pigment can leave residue in dead zones.
The grey 7736 colour system is likely to contain inorganic pigments such as carbon black, titanium dioxide, or mixed metal oxides in a polyethylene carrier. Inorganic pigment agglomerates increase viscosity, reduce tensile elongation, and can initiate premature failure at film gauge below 40 µm. Dispersion quality should be checked by pressure-rise filtration through screens of 100 mesh to 250 mesh, or by film optical inspection for grey streaks. If the pigment masterbatch is not fully homogenised, weld-line strength in injection-moulded parts may fall below the expected value for natural resin. The colour also influences melt temperature: carbon black absorbs heat, while titanium dioxide acts as a reflective filler. Differential scanning calorimetry on the compounded material is recommended before setting a melt profile.
The grey 7736 designation does not define pigment loading; it specifies a colour standard against which lot-to-lot variation is controlled. If exact colour matching is required, spectrophotometric checks with a D65 illuminant and 10° observer using CIELAB coordinates should be applied. Colour differences of ΔE* below 1.0 are often invisible; a shift greater than 1.5 may be perceptible in adjacent components. Because pigment loading can affect density and melt-flow rate, the certificate of analysis should list these values on the final compound, not only on the natural base resin.
Mechanical evaluation for incoming material should use compression-moulded or injection-moulded specimens prepared in accordance with ISO 1872-2:2007 and conditioned at 23 °C and 50 % relative humidity for at least 88 h. Tensile yield stress for metallocene LLDPE in this density region often falls between 10 MPa and 20 MPa, with elongation at break above 500 %. Flexural modulus typically lies below 500 MPa for uncoloured material; the grey pigment may increase modulus by 5–15 % depending on loading. These values are not lot-specific release data and must be replaced by the manufacturer’s certificate for Icorene 1761 GRY 7736.
Compliance verification for Icorene 1761 GRY 7736 should be driven by the supplier’s regulatory documentation. The following matrix identifies the core test or standard designations that converters often request.
| Standard or regulation | Scope | Documentation basis |
|---|---|---|
| ISO 1133-1:2022 | Melt mass-flow rate of thermoplastics | Certificate of analysis |
| ISO 1183-1:2019 | Density by immersion or gas pycnometry | Lot release data |
| ISO 527-2:2012 | Tensile yield stress and elongation at break | Moulded type 1A or 5A specimens |
| FDA 21 CFR 177.1520 | Olefin polymers for food contact | Supplier compliance declaration |
| EU No 10/2011 | Plastic food-contact materials and articles | Migration test report |
| REACH EC 1907/2006 | Registration, evaluation and authorisation | Extended safety data sheet |
Food-contact status for pre-coloured grades must account for the pigment system. The base resin may comply with FDA 21 CFR 177.1520, but the colourant and additives must also meet applicable clearances. Under EU No 10/2011, overall migration should be tested with food simulants appropriate to the intended use; colourants are not automatically covered by the base polymer authorisation. The supplier should provide a compliance statement for the specific GRY 7736 formulation. For non-food industrial use, REACH registration of the base polyethylene and any intentionally added substances must be documented in the safety data sheet.
In film applications the low-density metallocene backbone supports high puncture resistance and low-temperature flexibility. The product is not suitable for applications requiring high clarity because the grey 7736 colour displaces transparency. It is typically directed to tinted industrial films, carrier bags, agricultural covers, or injection-moulded closures where a pre-compounded grey eliminates dry colour mixing. When the material is converted on a cast-film line, the cooling-roll stack should be set to 30–50 °C for thickness stability. For injection moulding, the clamping force requirement follows standard LLDPE conditions; however, the narrow molecular weight distribution of the metallocene resin can require slightly higher injection velocity to fill thin-walled sections.
For flexible packaging, the metallocene architecture generally reduces seal initiation temperature by 5–10 °C relative to a Ziegler–Natta LLDPE of similar density and MFR. The narrower melting distribution creates a sharper heat-seal transition, which can improve line-speed stability on vertical form-fill-seal equipment. However, the grey 7736 colour may absorb heat differently in sealing bars. It is advisable to map seal strength across 100 °C to 150 °C with 0.2 s dwell and 0.5 MPa jaw pressure before production. Published data for this specific pre-coloured configuration is limited in public technical literature, so laboratory trials are required.
In injection moulding, the material’s narrow molecular weight distribution reduces shear thinning; filling thin-walled components may require injection pressures higher than those used for conventional LLDPE. Mould temperature generally ranges from 10 °C to 40 °C; melt temperature is typically 200 °C to 240 °C; injection speed should be increased in steps to avoid jetting while ensuring full filling. The grey pigmentation makes weld lines more visible; melt temperature uniformity and vent depth of 0.01–0.03 mm should be maintained. Cycle time is controlled by cooling time, which must be based on part thickness rather than resin type.
The base polyethylene in Icorene 1761 GRY 7736 is not inherently weather-stable unless an appropriate UV stabilisation package is included. The grey pigmentation may provide partial light screening; carbon black at sufficient loading can improve UV resistance, but titanium dioxide and organic pigments do not guarantee oxidative stability. Long-term heat ageing should be evaluated by ISO 188:2023 or ISO 4577:2019 at temperatures below the melting region. If the part is exposed to hot water or steam above 80 °C, extraction of antioxidants can accelerate embrittlement. The material should not be used for continuous service above its Vicat softening temperature, and it is not a replacement for cross-linked polyethylene or polypropylene in pressurised hot-water systems.
Differences from other products are most evident in seal and toughness performance. Compared with a conventional butene-based Ziegler–Natta LLDPE of equal density, the metallocene product is expected to show more uniform sealing and lower seal initiation temperature. Compared with high-pressure LDPE, it has lower melt strength and lower optical clarity but higher dart impact and puncture resistance. Compared with single-site plastomers or very low-density polyethylenes, its modulus remains closer to standard LLDPE, which maintains stiffness in film structures. Because the grey 7736 version is a pre-coloured compound, it differs from natural Icorene or masterbatch-diluted versions by eliminating the need for a colour additive feeder, but it also reduces formulation flexibility and requires dedicated material handling.
Compared with LyondellBasell’s own natural Icorene grades, the GRY 7736 version carries an additional colour concentrate or pre-compounded pigment package, so its oxidative induction time and melt stability may differ. If the natural grade is supplied with an external masterbatch at the converter’s dosing unit, the same colour match can be achieved with more formulation flexibility but lower lot-to-lot consistency than the pre-coloured variant. The pre-coloured route reduces housekeeping and prevents dust generation but locks the converter into a fixed pigment loading and carrier fraction.
Recycling stream contamination with polypropylene or HDPE can shift the melt freezing point and reduce dart impact. The material should not be dry-blended with high levels of regrind without property testing. In industrial operations, post-industrial regrind of the same GRY 7736 material can typically be re-incorporated up to 20–30 %, but the exact limit depends on heat history and film property requirements.
Operational boundaries should be observed. Storage below 50 °C and protected from direct sunlight reduces pre-processing oxidation. If pellets are exposed to relative humidity above 60 %, pre-drying at 80 °C for 2–4 h may be required, particularly for injection moulding, because the colour carrier and pigment surface can adsorb moisture. Avoid blending with amine-based nitrogen-containing additives, which can antagonise hindered phenolic antioxidants. Avoid residence times longer than 15 minutes at melt temperatures above 230 °C, and do not process at barrel temperatures above 250 °C without documented purge and degradation control. These boundaries follow general metallocene LLDPE processing practice; the manufacturer’s lot-specific instructions remain authoritative for Icorene 1761 GRY 7736.