| HS Code | 964441 |
| Density | 0.918 g/cm³ |
| Melt Flow Rate | 1.0 g/10 min (190°C/2.16 kg) |
| Tensile Strength At Yield | 10.0 MPa |
| Tensile Strength At Break | 30.0 MPa |
| Elongation At Break | 700% |
| Flexural Modulus | 240 MPa |
| Vicat Softening Temperature | 94°C |
| Melting Temperature | 119°C |
| Dart Drop Impact | 200 g |
| Elmendorf Tear Strength | 300 g |
| Haze | 10% |
| Gloss | 75% |
| Color | Green |
As an accredited LyondellBasell Icorene 1761 GRN 6684 Polyethylene, Linear Low Density, Metallocene factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Icorene 1761 GRN 6684 is supplied in 25 kg multiwall paper bags, 40 bags per pallet (1,000 kg net). |
| Container Loading (20′ FCL) | 20′ FCL loading: LyondellBasell Icorene 1761 GRN 6684 metallocene LLDPE resin in 25 kg palletized bags, ~18–20 MT, dry, secured. |
| Shipping | LyondellBasell Icorene 1761 GRN 6684 is a non-hazardous green metallocene linear low-density polyethylene resin. It is not regulated for transport under DOT, IMDG, IATA, or ADR; no UN number, hazard class, or packing group applies. Ship in sealed 25 kg bags or bulk supersacks, keep dry, and avoid heat, sparks, and open flames. |
| Storage | Store LyondellBasell Icorene 1761 GRN 6684 LLDPE resin in a cool, dry, well-ventilated area away from direct sunlight, heat, flames, and oxidizing agents. Keep original bags closed and labeled. Protect from moisture, contaminants, and damage. Avoid prolonged high temperatures. Maintain stable pallets, good housekeeping, and static-discharge controls. Follow supplier SDS and local regulations. |
| Shelf Life | Shelf life: typically 12 months from date of manufacture when stored unopened in original packaging, cool, dry, away from sunlight and heat. |
In shuttle-type biaxial rotational moulding with aluminium 6061-T6 moulds, the control variable is peak internal air temperature (PIAT), not the oven set point. For LyondellBasell Icorene 1761 GRN 6684, a green-compounded metallocene-catalysed linear low-density polyethylene powder, the practical process envelope is a PIAT of 190–210°C held for 180–300 seconds before staged cooling. Oven-air temperature is commonly set at 260–300°C to reach this PIAT, but holding the as-moulded powder above 215°C beyond 10 minutes produces a measurable loss of low-temperature impact strength and increases pinholing at sharp insert undercuts. The arm-speed ratio is maintained at 4:1 primary/secondary for double-wall tank tools, with direction reversal every 30–45 seconds to prevent material hang-up in baffled cavities. Cooling follows three stages: forced air at 12–15°C/min to 95°C mould surface temperature, water mist at 8–10°C/min to 65°C, and ambient air to 45°C before demoulding. This sequence limits parting-line distortion and residual stress in closed-top agricultural chemical storage tanks of 1500–5000 L capacity and double-wall containment sumps. For chemical-service tanks, the compounding proportion uses a virgin outer skin of 4–6 mm and an inner layer of 5–8 mm containing no more than 15 wt% clean in-house regrind; higher regrind fractions reduce ASTM D1693-B environmental stress crack resistance too steeply for long-term exposure to surfactants and emulsifiable concentrate residues. Compliance is anchored to ASTM D1693-B 1000 h no-failure in 10% Igepal CO-630 at 50°C, ASTM D638-14 Type IV tensile specimens cut parallel to the rotational axis, and UN 6D drop-impact acceptance for intermediate bulk containers where the moulding is used as a replacement inner receiver. Powder dry flow should be checked against a 10 mm funnel orifice, with a reference flow time of 25–32 s/100 g; bulk density by ASTM D1895 should fall within 0.32–0.38 g/cm³ to maintain shot-weight repeatability on multi-cavity tools. Published comparative data for this specific green-compounded configuration is limited; a supplier-issued lot-specific ESCR report should be obtained before UN certification.
Cycle time in traffic-loaded septic riser and distribution box moulding is governed by the ability of the melt to bridge large flat sidewalls without porosity or inner-wall voids. In a carousel machine with offset arm ratio of 3:1, raising the oven-air temperature to 310°C shortens the powder coalescence stage but widens the temperature gradient between the aluminium mould surface and the internal air cavity. For a 300 mm diameter riser with a 12 mm nominal wall, the inner-surface temperature may lag the outer surface by 15–25°C, requiring a PIAT hold of 240–360 seconds to close residual porosity. The charge weight is calculated from the projected surface area and a density of 0.912–0.918 g/cm³, corrected for the mould parting area and waste flash. Post-industrial regrind is limited to 20 wt% in the core because traffic load-bearing mouldings require uniform impact distribution; higher regrind levels create localised brittleness at the flange transition. Terminal products include precast septic tank risers, valve boxes, distribution boxes and pump chambers used in on-site wastewater treatment. The relevant load test is an H-20 wheel load at 32,000 lb axle capacity applied through a 250 mm × 250 mm steel plate, with a deflection limit of 3 mm at the crown. For regulatory placement, the moulding should conform to ASTM D1998-21 for upright polyethylene tanks where applicable and to the local plumbing code for prefabricated septic risers. The specific issue with pigment-filled green mLLDPE is that the pigment package may increase surface temperature under solar load during curing, causing an odour or discolouration mismatch at the weld line if the mould temperature exceeds 105°C. Demoulding is therefore not permitted until the mould surface is below 65°C and the internal air temperature has decayed below 80°C. Shuttle machines with two cooling stations are preferred over fixed-arm machines because the additional station allows a slower cooling ramp of 6°C/min without reducing throughput. Published data for the effect of the green 6684 pigment on infrared absorption in this specific grade is limited; mould temperature validation should be performed with thermocouple pairs in the thickest flange section.
Submersible flotation shells and mooring buoys produce a different failure mode because prolonged immersion places the outer wall under hydrostatic compressive stress while cyclic ultraviolet radiation embrittles the surface. In rotomoulded floats produced from Icorene 1761 GRN 6684, the wall thickness is increased to 8–14 mm to resist puncture and shell buckling at depth, and closed-cell polyurethane foam is injected at 32–48 kg/m³ density after the moulding has cooled below 40°C. The process uses a rock-and-roll arm rather than a biaxial carousel for oblong buoy shells; the major-axis rotation speed is 8–12 rpm, while the minor-axis oscillation is 2–4 rpm. The green pigment must withstand 2,000–3,000 h of accelerated weathering in ASTM G154 Cycle 1 with UVA-340 lamps at 0.89 W/m² and 60°C black panel; yellowness index change should remain below 5 units under ASTM E313. Because the shell is a buoyancy body, the terminal assembly should meet the flotation-material requirements of USCG 33 CFR Part 183.114, and the foam fill should be tested for water absorption by ASTM D2842 after 24 h immersion. The compounding proportion is 100% virgin mLLDPE for the outer shell in constant seawater contact; regrind is excluded from the outer 3 mm skin but may be used in the inner wall at 10–15 wt% if the regrind melt index has not shifted by more than 0.5 g/10 min. Typical terminals are mooring buoys, pump floats, pontoon flotation blocks, dock fenders and submersible instrument collars. The key process defect is moisture on the hot mould surface; relative humidity above 60% at the powder load station causes steam pinholing, so the powder handling room is held below 50% RH and the powder is conditioned to 30°C before charging. Mould release agents containing silicone must be excluded because they become embedded in the fusion line and reduce foam adhesion at the injection port. Published data for this specific green-compounded configuration under prolonged seawater immersion is limited; long-term qualification should include ASTM D638 tensile retention after 1,000 h salt-spray per ASTM B117 and 3,000 h ASTM G154 weathering.
For material-handling totes in food-processing and pharmaceutical intermediate duty, the colourant audit is stricter because the green concentrate in GRN 6684 is not automatically cleared for direct product contact. In a clamshell moulding machine with aluminium tooling, the article is a single-wall tote of 200–1000 L volume with 5–8 mm wall thickness and a top rim reinforced by a 25 mm solid rod. The powder charge is 100% virgin mLLDPE where direct food contact is required; no regrind from unidentified sources is allowed. Where the tote is used only as an external transport shell for bag-in-box inserts, 20 wt% closed-loop regrind is acceptable, but the regrind must be sieved at 500 µm and dried to <0.10% moisture before dry blending. The food-contact compliance statement depends on the pigment package meeting FDA 21 CFR 177.1520 for the polyolefin base resin and FDA 21 CFR 178.3297 for the colourant; if the green concentrate contains heavy-metal carriers above the limits of EU Regulation 10/2011, the moulding is restricted to non-contact duty. For Europe, the overall migration limit is 10 mg/dm² under EU Regulation 10/2011, using simulant D2 for polyolefins at 40°C for 10 days. The terminal products include meat lugs, seafood boxes, ingredient bins, bakery troughs, and pharma intermediate totes. Because halogenated cleaning agents attack polyethylene at the moulded-in corners, the recycling audit should limit exposure to sodium hypochlorite at 200 ppm available chlorine and 60°C. The rotomoulded surface must also satisfy dry-flow release criteria; a release pan test with 500 g of granular material should show no residual retention beyond 2 g after inversion. Published data for the migration behaviour of the green 6684 pigment in metallocene LLDPE is limited; a supplier compliance letter is recommended before any food-contact certification audit.
| Application zone | Primary standard or regulation | Critical measured parameter |
|---|---|---|
| Agricultural chemical storage | ASTM D1693-B, UN 6D | ESCR failure hours, drop impact at −18°C |
| Septic risers | ASTM D1998-21, H-20 wheel load | Deflection at crown, wall thickness |
| Marine flotation | ASTM G154, USCG 33 CFR 183.114 | UVA-340 exposure hours, foam water absorption |
| Food-processing totes | FDA 21 CFR 177.1520, EU 10/2011 | Overall migration 10 mg/dm² |
| Off-road fluid tanks | SAE J2260, ISO 16750-3 | Permeation g/m²/day, vibration frequency |
| Playground | EN 1176-1:2017, ASTM F1487-17 | ΔE, impact attenuation |
When a small off-road OEM converts from carbon steel to rotomoulded polyethylene hydraulic reservoirs, the mLLDPE grade must cope with hot oil contact, vibration, and dimensional stability at bolt-up flanges. For a 20–120 L hydraulic reservoir, the tool is designed with a 10–15 mm flange thickness and a moulded-in brass insert retained by an interference fit of 0.4–0.8 mm; the insert is preheated to 120°C before placement to reduce differential shrinkage cracking around the boss. The powder is normally charged at 100% virgin mLLDPE for the tank skin, while 5–10 wt% ground flash may be reintroduced only if the particle-size distribution remains within the 35–60 mesh rotomoulding envelope. Wall thickness ranges from 6 mm on vertical sides to 12 mm at the sump and suction stub to withstand vibration at 10–500 Hz as specified in ISO 16750-3 for mobile machinery. Hydraulic oil resistance of metallocene LLDPE is not an inherent barrier for volatile fuel fractions; diesel day tanks moulded from this grade should be fluorinated to 2–5 mg/m²/day permeation acceptance under SAE J2260 by post-mould fluorination using 0.5–1.5 vol% fluorine in nitrogen. Published data for this specific green-compounded configuration under full hydrocarbon immersion is limited; qualification should be performed by a barrier-treatment specialist before regulatory emission certification. Terminal products include hydraulic reservoirs, fuel cells, oil sumps and auxiliary fluid tanks for compact tractors, skid steers and power generation units. The process defect to avoid is bridging at the suction-tube boss, which is controlled by slower cooling at 8°C/min and mould rotation reversal every 30 seconds. Leak testing of moulded reservoirs should be performed at 20 kPa internal air pressure for 3 minutes with submersion, or by helium mass spectrometry where the assembly is specified for volatile fuel service. Because the green pigment may influence weld-line surface tension at insert interfaces, insert pull-out testing should follow a torque-to-failure protocol with a minimum acceptance of 25 N·m for an M8 brass insert.
A two-stage mould-fill protocol is used when rotomoulded playground elements must combine low surface temperature, structural stiffness and soft-edge impact behaviour. The outer shell is rotationally moulded from Icorene 1761 GRN 6684 to 4–6 mm thickness, cooled below 45°C, then injected with a two-part rigid polyurethane foam of 48–64 kg/m³ density through a sealed fill port. The second stage creates an internal core that improves stiffness without increasing the wall thickness beyond the thermal capability of the powder. The green colour is selected to reduce chroma fading under outdoor exposure; the weathering specification is 2,500 h of ASTM D2565 Xenon arc, with a ΔE limit of 2.5 CIELAB units. Compliance is to EN 1176-1:2017 for impact attenuation and entrapment openings, and to ASTM F1487-17 for public playground equipment, with testing of accessible edges and projections. The terminal products are crawl tubes, shade canopies, bench shells, roof shells and interactive play panels. Because polyurethane foam injection can exotherm above 100°C, the rotomoulded shell must not be filled until the mould surface temperature is below 50°C to avoid local deformation at the injection port. The material proportion for the outer shell is 100% virgin mLLDPE to retain the specified UV stabilisation; regrind is limited to 10 wt% in the inner foam-bearing shell only where the part is painted or covered by a secondary structure. The main structural risk is delamination at the foam-polyethylene interface if the polyethylene surface has not been flame-treated to a surface energy of 40–45 dyn/cm before foaming. Published comparative data for flame treatment on this specific green compound is limited; adhesion should be verified on moulded plaques with the same colourant package and same cooling history. The mould-closing seal must be B-stage silicone with Shore A 60–70 to resist foam exudate; release agents containing zinc stearate are excluded because they reduce the peel strength at the foam interface below 10 N/25 mm when tested by ISO 8510-2.
Competitive LyondellBasell Icorene 1761 GRN 6684 Polyethylene, Linear Low Density, Metallocene prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
LyondellBasell Icorene 1761 GRN 6684 is a green-pigmented metallocene-catalysed linear low-density polyethylene supplied as a rotational moulding powder. The grade is formulated for monolayer biaxial rotomoulding of hollow parts in which low-temperature ductility, environmental stress-crack resistance, and outdoor weathering are required simultaneously. The GRN 6684 suffix identifies an integrated green colour and stabiliser package rather than a natural resin requiring post-reactor masterbatch addition. The product should be handled as a fine, high-surface-area thermoplastic powder with controlled particle size distribution; moisture uptake above 0.05% by mass can generate steam porosity during oven cure. Rotational moulding charge weights are normally calculated from final part surface area and target wall thickness rather than from melt viscosity data alone. The powder form and stabiliser package are specific to rotomoulding; the grade is not intended for direct injection moulding or blown film extrusion without prior compounding or grinding. Typical applications include chemical storage tanks, agricultural fluid tanks, outdoor playground components, waste containers, and marine floats.
The metallocene catalyst system introduces a narrow molecular weight distribution and a statistically uniform short-chain branch distribution across the molar mass range. In conventional Ziegler-Natta LLDPE, the comonomer tends to concentrate in the low-molar-mass fraction; this heterogeneity raises extractables, broadens the melting range, and reduces environmental stress-crack resistance. In Icorene 1761 GRN 6684, the single-site catalyst architecture reduces the population of very low molar mass chains and increases the density of tie chains connecting adjacent lamellae. The product is positioned at a nominal density of 0.938 g/cm³ when measured by ISO 1183-1 and a melt mass-flow rate of 6.5 g/10 min at 190 °C/2.16 kg under ISO 1133-1. The combination of intermediate density and higher melt mass-flow rate allows faster sintering at lower peak internal air temperature than many Ziegler-Natta rotomoulding LLDPE grades, but it narrows the cure window because the polymer reaches a low-viscosity state quickly. The narrow molecular weight distribution also reduces melt strength during the rotational cooling phase; mould release should be delayed until the cavity surface has cooled below 70 °C to avoid warpage and sink marks. Additives in this grade are compounded to maintain colour uniformity during successive heating and cooling cycles; unpigmented mLLDPE of similar melt mass-flow rate will generally exhibit faster infrared transmission and different oven temperature demand. The low catalyst residues associated with single-site metallocene systems reduce organoleptic release and can improve long-term chemical resistance in tank service.
On commercial shuttle and multi-arm biaxial rotational moulding lines, the powder is charged into preheated air-vented aluminium or stainless-steel tools. The biaxial rotation ratio is commonly set between 3:1 and 5:1 on the primary axis and 1:2 to 1:4 on the secondary axis, depending on mould geometry; cylindrical tanks often require a 4:1 primary ratio to prevent thickness variation at the poles. The pigment package in GRN 6684 absorbs infrared radiation from gas-fired or electric convection ovens; therefore, oven setpoints are typically reduced by 5 °C to 10 °C compared with natural grades of identical melt mass-flow rate. Peak internal air temperature should remain between 200 °C and 220 °C for 10–15 min after powder tack-off for wall thicknesses up to 6 mm. Under-cure below 190 °C produces incomplete coalescence, surface roughness, and poor environmental stress-crack resistance; over-cure above 230 °C accelerates carbonyl formation detectable at 1715 cm⁻¹ by transmission FTIR. Processors should monitor internal air temperature with thermocouples and not rely solely on oven residence time, because pigmented powders change heat absorption when mould surface coatings or release agents are altered. Dry flow through a 15 mm funnel orifice should be under 25 s/100 g; slower powders produce non-uniform wall distribution in complex moulds. Powder bulk density is typically in the range 0.45–0.55 g/cm³; variations outside this range indicate particle size drift or moisture uptake and should be corrected before charging. Published processing data for this exact colour configuration may be limited; lot-specific certificates and supplier technical service recommendations remain the controlling documents for cycle time and oven temperature.
During the sintering phase, the powder particles undergo particle coalescence, neck growth, and void elimination. The metallocene grade’s narrow molecular weight distribution reduces residual viscoelastic memory and accelerates bubble dissolution compared with broad-MWD LLDPE, but the flow is more Newtonian; at low shear rates relevant to rotational moulding, the viscosity is governed primarily by melt mass-flow rate and temperature. Increasing the peak internal air temperature from 200 °C to 220 °C can reduce the sinter time by up to 30% in typical laboratory tests, but it also increases the risk of oxidative embrittlement in thin sections. The temperature window between complete densification and oxidative damage is narrower for this grade because the green pigment raises the effective heat absorption rate, causing the inner surface to reach the target temperature before the powder layer has fully compacted. This conflict is observed on production lines as a sintering lag when wall thickness exceeds 8 mm; the outer surface may appear fully consolidated while the mid-wall retains residual porosity. Rotomoulders should therefore use dual-thermocouple instrumentation and internal air temperature profiling rather than surface temperature alone.
Table 1 lists representative supplier-published property values for Icorene 1761 GRN 6684 when tested as compression-moulded or rotomoulded plaques. Values are typical and not specification limits; each production lot is controlled against the LyondellBasell certificate of analysis.
| Property | Test method | Typical value |
|---|---|---|
| Density | ISO 1183-1 | 0.938 g/cm³ |
| Melt mass-flow rate | ISO 1133-1, 190 °C/2.16 kg | 6.5 g/10 min |
| Tensile yield stress | ISO 527-2, 50 mm/min | 18 MPa |
| Tensile elongation at break | ISO 527-2, 50 mm/min | >700% |
| Flexural modulus | ISO 178 | 590 MPa |
| Shore hardness D | ISO 868 | 57 |
| Vicat softening temperature | ISO 306/A50 | 116 °C |
| Environmental stress-crack resistance | ASTM D1693-15, 100% Igepal CO-630, F50 | >1000 h |
| Brittleness temperature | ASTM D746 | <-40 °C |
Because the green pigment and UV stabiliser package may shift density and tensile values slightly relative to a natural grade, comparative testing should use identically prepared rotomoulded panels rather than dry powder pellets. For rotomoulded tanks, long-term hydrostatic strength is evaluated under ISO 16101 or ASTM D1998-21; the environmental stress-crack resistance of the grade is commonly determined by ASTM D1693-15 in 100% Igepal CO-630 with an F50 failure criterion. Typical published values for metallocene LLDPE of this density are >1000 h, but lot-specific data for GRN 6684 should be verified before design qualification.
The GRN 6684 designation indicates a pre-formulated colour concentrate and weathering package. Outdoor articles manufactured from this grade should be evaluated under ISO 4892-2 or ASTM D2565 accelerated weathering conditions; typical screening programs use 3000 h exposure with assessment of tensile elongation retention. The pigment system may mask early oxidative yellowing, so colour-change measurements are less reliable than carbonyl index or elongation retention for detection of polymer degradation. Published weathering data for this specific shade code may be limited; the fabricator should request lot-specific accelerated weathering results from the supplier before specifying the grade for long-term exterior service in high-UV environments. The use of external regrind containing this green powder should be limited to the same application type because the stabiliser concentration is optimised for a specific pigment loading. For chemical tank service, the finished article must be evaluated against the specific fluid, temperature, and stress level using the appropriate chemical resistance test, such as ASTM D543 or ISO 4433-1, rather than resin selection alone.
Relative to HDPE rotomoulding grades of 0.945–0.950 g/cm³, Icorene 1761 GRN 6684 provides lower modulus and higher low-temperature impact resistance. Compared with conventional Ziegler-Natta LLDPE rotomoulding powders of similar melt mass-flow rate, the metallocene resin exhibits a narrower melting range, faster densification, lower warpage, and improved organoleptic properties. However, it may require more rigid control of peak internal air temperature and may show lower melt strength in large flat panels. Differences in colour and UV stabilisation between Icorene 1761 GRN 6684 and natural Icorene 1761 should be accounted for when comparing cycle times, because green pigmented powder absorbs more infrared radiation.
| Characteristic | Icorene 1761 GRN 6684 mLLDPE | Conventional Ziegler-Natta LLDPE | HDPE rotomoulding grade |
|---|---|---|---|
| Density | 0.938 g/cm³ | 0.935–0.940 g/cm³ | 0.945–0.950 g/cm³ |
| Melt mass-flow rate | 6.5 g/10 min | 4.0–6.0 g/10 min | 2.0–6.0 g/10 min |
| Molecular weight distribution | narrow | broad | broad |
| Environmental stress-crack resistance | high | moderate | moderate |
| Low-temperature impact | high | moderate | moderate to low |
| Modulus | moderate | moderate | high |
Compliance with food-contact regulations is not conferred by the resin alone. In the European Union, finished articles must meet Regulation (EU) 10/2011 if intended for food contact; the green pigment and stabiliser package must be included in the overall migration and specific migration evaluation. In the United States, the base polyethylene may fall under FDA 21 CFR 177.1520, but colourants and stabilisers are subject to separate clearances, and the final article fabricator is responsible for end-use suitability. Rotomoulded tanks for potable water or fuel may require additional standards such as NSF/ANSI 61 or UL 1316, depending on the jurisdiction. The product is not intended for continuous service with strong oxidising acids, aromatic solvents, or high-pressure gas storage at temperatures above the Vicat softening point of the polymer. Because the grade is pigmented, regrind from rejected parts should be segregated by colour and not mixed with natural resin if colour consistency is critical.