| HS Code | 157452 |
| Density | 0.917 g/cm³ |
| Melt Mass Flow Rate | 1.6 g/10 min (190 °C/2.16 kg) |
| Melting Temperature | 118 °C |
| Vicat Softening Temperature | 94 °C |
| Tensile Strength At Yield Md | 9.0 MPa |
| Tensile Strength At Yield Td | 8.0 MPa |
| Tensile Strength At Break Md | 35.0 MPa |
| Tensile Strength At Break Td | 30.0 MPa |
| Elongation At Break Md | 600 % |
| Elongation At Break Td | 700 % |
| Flexural Modulus | 200 MPa |
| Dart Drop Impact | 150 g |
| Elmendorf Tear Strength Md | 200 g |
| Elmendorf Tear Strength Td | 400 g |
| Haze | 6 % |
| Gloss 45 | 80 |
| Coefficient Of Friction | 0.2 |
As an accredited LyondellBasell Icorene 1761 BUE 5581 Polyethylene, Linear Low Density, Metallocene factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Supplied in 25 kg polyethylene bags, palletized, stretch-wrapped; typically 55 bags per pallet (1,375 kg). |
| Container Loading (20′ FCL) | 20′ FCL holds approximately 18–20 metric tons of palletized 25 kg bags of Icorene 1761 BUE 5581 metallocene LLDPE. |
| Shipping | LyondellBasell Icorene 1761 BUE 5581 is typically shipped as non-hazardous metallocene linear low-density polyethylene resin pellets. Standard packaging includes 25 kg PE bags or bulk bags on pallets, in dry containers or trucks. Store and transport away from moisture, heat, and direct sunlight. No special hazardous-materials handling required. |
| Storage | Store in a cool, dry, well-ventilated area away from direct sunlight, heat, and ignition sources. Keep material in original sealed packaging, palletized, and off the floor to prevent moisture and contamination. Avoid prolonged UV exposure and excessive stacking. Maintain ambient storage temperatures, observe good housekeeping, and follow first-in, first-out stock rotation and the supplier’s SDS. Do not store near strong oxidizers. |
| Shelf Life | Shelf life is typically 24 months when stored in original unopened packaging, cool, dry, away from direct sunlight and moisture. |
In rotational moulding, Icorene 1761 BUE 5581 is processed as a dry-flowing powder with a manufacturer-listed nominal density of 0.917 g/cm³ when determined by ISO 1183-1:2019 and a nominal melt flow rate of 6.0 g/10 min when measured under ISO 1133-1:2022 at 190 °C with a 2.16 kg load. The powder is converted on multi-arm carousel rotomoulding machines with forced-convection oven temperatures between 260 °C and 315 °C. The peak internal air temperature, commonly abbreviated as PIAT, is held in the 190–210 °C range to obtain complete particle coalescence while avoiding oxidative chain scission at the inner wall. For stationary chemical storage vessels, the governing compliance document is ASTM D1998-21, which sets requirements for minimum wall thickness, hydrostatic integrity, venting, and polyethylene property verification. The formulation for outdoor chemical storage tanks consists of 100 phr of the metallocene LLDPE powder, 0.2–0.6 phr of a hindered amine light stabiliser or UV stabiliser package, 0.05–0.15 phr of a hindered phenolic antioxidant, and 0.5–2.0 wt% of carbon black or an approved chemical-resistant pigment masterbatch. Powder particle size distribution is controlled between 200 μm and 500 μm by laser diffraction or sieve analysis, with fines below 150 μm limited to 10 wt% because excessive fines migrate toward the mould surface during tackification and produce microvoiding. The downstream production sequence includes cold powder charging, biaxial rotation, oven sintering, forced-air or water-mist cooling, and demoulding below 80 °C. Overfiring above 210 °C PIAT or localised oven hot spots above 315 °C causes chain scission, discolouration, and a measurable loss of low-temperature impact resistance. Incomplete densification below 190 °C leaves weld-line porosity at the powder particle interfaces, which can initiate environmental stress cracking in contact with surfactants or oxidising media. The terminal product category includes cylindrical vertical chemical storage tanks, double-wall containment vessels, and corrosion-resistant dosing cabinets used in water treatment, metal finishing, and agricultural chemical storage.
| Parameter | Test Method or Equipment | Nominal Value or Range |
|---|---|---|
| Nominal density | ISO 1183-1:2019 | 0.917 g/cm³ |
| Nominal melt flow rate | ISO 1133-1:2022, 190 °C, 2.16 kg | 6.0 g/10 min |
| DSC melting peak | ISO 11357-3 | 120–125 °C |
| Rotomoulding oven set temperature | Forced-convection multi-arm carousel | 260–315 °C |
| Peak internal air temperature | Internal air thermocouple | 190–210 °C |
| Demoulding temperature | Infrared pyrometer | <80 °C |
| Powder particle size | Laser diffraction or sieve analysis | 200–500 μm |
The rotational lining of carbon steel pipework in chemical transfer plants is an established conversion route for metallocene LLDPE powders where a fused polyethylene liner of 2–6 mm thickness provides corrosion isolation without fabricating an all-polyethylene pressure boundary. In this application, substrate preparation follows ISO 8501-1:2007 surface cleanliness grade Sa 2½, with the blast-cleaned anchor profile controlled to 50–100 μm and verified by ISO 8503-2. The powder charge is introduced after the steel spool reaches 250–300 °C, and the biaxial rotation sequence is held at an internal material temperature of 190–210 °C until gelation and void elimination are confirmed on a sacrificial witness panel. The formulation consists of 100 phr Icorene 1761 BUE 5581, carbon black dispersion at 0.5–1.5 wt%, and zinc stearate acid scavenger limited to <0.05 wt% to avoid interface plate-out. Amine-based adhesion promoters are excluded because amine species can migrate to the steel-polymer interface and reduce peel strength under hot-wet exposure. Post-mould cooling is performed with forced air rather than direct water quench to reduce differential shrinkage between the steel wall and the liner. Finished product types include lined pipe spools from DN40 to DN300, lined elbows, tees, and dip pipes. Operational limitations include a maximum continuous service temperature below 60 °C in aggressive chlorinated media, because peel strength declines progressively when the steel-liner interface reaches 60–70 °C. Published data for this specific grade in rotational pipe lining is limited outside the manufacturer’s processing recommendations, but the cycle parameters are consistent with standard polyethylene rotomoulding practice.
The food-contact conversion path for this metallocene LLDPE grade is governed by olefin-specific compliance rather than generic resin certification. Under FDA 21 CFR 177.1520, the base polymer is evaluated for extractables using the food simulants and end-test criteria applicable to olefin polymers; under EU Regulation 10/2011 Annex I, overall migration is controlled to 10 mg/dm² with simulant selection based on the intended food type and contact temperature. In rotomoulded food transport boxes, the formulation comprises 100 phr base resin, food-grade silicone slip additive at 0.1–0.3 phr, and white titanium dioxide masterbatch at 1.0–2.0 wt%. The masterbatch carrier is selected from the same metallocene LLDPE chemistry to avoid a discontinuous rheological response during oven sintering. Processing is conducted at oven temperatures of 260–300 °C, with peak internal air temperature held between 190 °C and 205 °C to minimise oxidative degradation at the inner surface. Prolonged cycles above 205 °C generate polar oxidation products that can raise migration values under polar food simulants. The moulded parts are cooled to below 60 °C before ejection to reduce warpage on large flat sidewalls. Terminal products include returnable dairy crates, insulated fish and seafood transport totes, and intermediate bulk containers for liquid food ingredients. External mould release agents are excluded from this process because they contaminate the polymer surface and complicate food-contact compliance testing under FDA 21 CFR 177.1520.
Masterbatch producers operating twin-screw compounding lines utilise Icorene 1761 BUE 5581 as a carrier matrix when the target pelletised masterbatch is intended for subsequent film, extrusion coating, or injection moulding dilution. The carrier loading is typically 70–80 wt%, pigment or additive content is 20–30 wt%, and processing stabilisers are added at 0.5–2.0 wt% of the masterbatch total. The compounding step is performed on a co-rotating twin-screw extruder with L/D 40:1 and a temperature profile from 180 °C at the feed throat to 230 °C at the die plate. Melt pressure is maintained below 80 bar to limit pigment agglomerate formation in the screen pack. The screw configuration uses distributive mixing elements rather than aggressive kneading blocks because the metallocene LLDPE matrix has a narrow melting interval and is sensitive to excessive shear heating. Compliance is limited to REACH Regulation (EC) No 1907/2006 Annex XVII restrictions on cadmium- and lead-based pigments, RoHS Directive 2011/65/EU for electrical and electronic applications, and ISO 9001 batch traceability. Final product types are pelletised colour masterbatches and additive masterbatches for polyethylene film, extrusion coating, and injection moulding. Published data for this specific grade as a masterbatch carrier is limited; plant-scale let-down trials are used to confirm dispersion because the pigment dispersion threshold varies with aggregate size and base resin melt index.
In low-emission automotive interior compounding, the metallocene LLDPE powder is metered as a ductility modifier in polypropylene-based thermoplastic olefin formulations at 10–25 wt%. The compound is produced on a twin-screw extruder with L/D 44:1, side feeding of 15–20 wt% talc, and a barrel temperature profile of 180–220 °C. The reduced crystallinity of the metallocene LLDPE modifies low-temperature impact without introducing the high extractable load associated with certain heterophasic ethylene-propylene rubbers. Volatile content is controlled by VDA 278:2011 VOC and FOG limits, and odour is tested according to VDA 270; REACH Regulation (EC) No 1907/2006 applies to restricted plasticisers and stabilisers. The additive package for an original equipment manufacturer interior substrate typically includes a phosphite antioxidant at 0.05–0.10 wt%, hindered amine light stabiliser at 0.10–0.30 wt%, and acid scavenger below 0.05 wt% to avoid plate-out on injection mould surfaces. The downstream process is high-speed injection moulding with clamp force from 500 to 1,600 tonnes, melt temperature 210–230 °C, and mould surface temperature 30–50 °C. Terminal product types include instrument panel retainers, door panel substrates, centre console rear shells, and seat side trim panels. Processing conflicts arise when the powdered LLDPE fraction exceeds 25 wt% because the compound then exhibits a measurable reduction in heat distortion modulus and a higher linear thermal expansion mismatch with talc-filled polypropylene.
Production-scale rotomoulding of waste-handling containers to EN 840-2 utilises Icorene 1761 BUE 5581 in monolayer or multilayer wall sections with wall thickness from 3 mm to 5 mm. The formulation for a two-wheeled container comprises 100 phr base resin, UV stabiliser at 0.1–0.4 phr, carbon black or dye masterbatch at 0.5–1.5 wt%, and antioxidant at 0.05–0.15 phr. The rotomoulding cycle is run on a biaxial carousel with oven temperature 260–300 °C, peak internal air temperature 190–205 °C, and forced-air cooling to 70 °C before demoulding. Dimensional conformity is verified according to EN 840-2, and tensile property measurement is conducted according to ISO 527-2. Product types include 120 L and 240 L two-wheeled bins, lids, and recycling containers. Operational limitations apply when processing thick sections: if the oven temperature is increased above 300 °C to shorten cycle time, the inner wall can retain excessive heat after demoulding and cause post-mould distortion on flat lid surfaces.
Competitive LyondellBasell Icorene 1761 BUE 5581 Polyethylene, Linear Low Density, Metallocene prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
LyondellBasell Icorene 1761 BUE 5581 is a metallocene-catalysed linear low density polyethylene supplied for extrusion-grade film applications. The suffix BUE 5581 may identify the stabilisation package, slip/antiblock system, and product form; exact values require lot-specific documentation. Grade-specific melt mass-flow rate should be verified according to ISO 1133-1:2022 at 190 °C and 2.16 kg, and density by ISO 1183-1:2019. Published aggregated data for this specific BUE 5581 configuration is limited; qualification work should therefore include incoming pellet analysis and film trials rather than reliance on generic published typical data. Typical film-application directions include cast stretch film, blown film, food-packaging laminates, frozen-food pouches, and heavy-duty sacks, but end-use suitability must be confirmed through target-line trials.
The grade designation does not by itself specify the α-olefin comonomer. In the Icorene range, the numerical sequence and suffix may identify density, melt-flow class, or additive formulation, but not whether butene, hexene, or octene is incorporated. A butene-based mLLDPE commonly displays lower seal initiation than a conventional C4 Z-N LLDPE, but may deliver lower puncture and tear toughness than an octene-based mLLDPE at equivalent density and melt index. Hexene- and octene-based grades generally shift the property balance toward higher hot-tack and dart impact, while also modifying stiffness and low-temperature flexibility. The exact comonomer used in Icorene 1761 BUE 5581 must therefore be taken from the supplier technical data sheet; comparative performance against other products cannot be reliably inferred from the product name alone.
In a conventional Ziegler-Natta LLDPE, multiple active species produce chains with different molecular weights and comonomer contents. That compositional heterogeneity broadens the crystallization range and increases the soluble fraction that can migrate during extraction testing. Metallocene catalysis replaces the multi-site population with a narrower active-site distribution. The ethylene/α-olefin insertion becomes more uniform, giving a more homogeneous short-chain branching distribution at the same overall density. The resulting film generally shows a lower seal initiation temperature, improved dart impact, and lower haze than a Z-N LLDPE of identical density and melt index. The distinction is not universal across all conversion lines because the narrow molecular weight distribution also reduces shear thinning. Processors who switch from Z-N LLDPE to mLLDPE often record higher melt pressure at the adapter, higher screw torque, and a different melt-fracture threshold, even when the melt index remains the same. In product comparisons, the shift should be treated as a change in rheological signature and not solely a change in solid-state properties.
Compared with high-pressure low density polyethylene, mLLDPE has a linear backbone without the long-chain branching that gives LDPE its melt strength and neck-in control. LDPE is therefore preferred where high melt extension and low neck-in are required, while mLLDPE is selected where tensile strength, puncture resistance, seal strength, and low-gauge film toughness are the primary targets. The difference is quantifiable through melt strength measurements, neck-in on a cast line, and standard tensile tests such as ISO 527-3:2018 or ASTM D882-12. When the end-use involves high-speed packaging, those differences must be evaluated in the same machine geometry; published data for this specific configuration is limited.
Incoming quality control for Icorene 1761 BUE 5581 should include pellet visual inspection, melt-flow and density confirmation, and additive package verification. Surface moisture introduced by humid storage may not be absorbed into the polymer backbone, but condensate above 0.05 % by mass can generate bubble defects or feed-throat slippage on a film line. A hopper dryer set at 80 °C for 0.5 h to 1.0 h can remove surface condensation, but prolonged high-temperature residence should be avoided. Because film friction and blocking are controlled largely by the slip and antiblock package rather than the base resin, a shift in additive loading can alter coefficient of friction measured by ASTM D1894-14 even when density and melt index remain unchanged. Product specifications should therefore include the additive certificate as well as the base polymer values. Lot-to-lot variance in pellet bulk density may also affect gravimetric feeder calibration and feed-throat mixing; bulk density should be measured if the material is blended with regrind or masterbatch at controlled addition rates.
On single-screw extrusion lines, the reduced shear sensitivity of mLLDPE can raise melt pressure and torque compared with Z-N LLDPE of equivalent melt index. This effect is commonly observed on a 60 mm smooth-bore extruder with 24:1 L/D at screw speeds above 80 rpm, where pressure transducer readings may increase by 10 % to 20 % when moving from a conventional Z-N LLDPE to a metallocene grade. If the die-lip shear stress surpasses the critical value for the melt, sharkskin and melt fracture can appear at outputs below the line’s mechanical maximum. The usual corrective action is to raise die and adapter temperature, widen the die gap, or reduce screw speed rather than adding backpressure. Starting cast-film profiles for narrow-MWD mLLDPE often use feed-zone temperatures of 175–190 °C, barrel temperatures from 200–250 °C, and die/adapter settings of 250–260 °C. In blown film, the lower melt strength relative to LDPE requires careful bubble geometry. Die gaps from 1.8 mm to 2.5 mm, higher frost-line heights, and internal bubble cooling are frequently used to maintain bubble stability at high blow-up ratios.
These values are line-dependent starting points, not fixed settings for Icorene 1761 BUE 5581. A capillary rheometry screen from 100 s-1 to 1000 s-1 can provide the shear-thinning index and apparent viscosity that correlate with screw torque and die pressure. The same data indicate whether a barrier screw, Maddock mixing head, or lower-compression screw design is appropriate. Narrow-MWD metallocene film grades can generate less shear heating than broad-MWD LLDPE, so mixing sections with tight clearances may be required to homogenize additive masterbatch without excessive melt residence time. Processing trials should record melt pressure, melt temperature at the die entrance, motor amperage, screw speed, film gauge, and die-lip smoke or plate-out, because those variables define the commercial operating window more reliably than laboratory melt index alone.
Qualification of metallocene LLDPE should be performed on the same film line and with the same testing laboratory that will accept the commercial product. The comparative table below shows typical envelopes for mLLDPE and Z-N LLDPE in thin-gauge film. These are general ranges used in supplier literature and do not replace the certificate of analysis for Icorene 1761 BUE 5581.
| Property | Test Method | Typical mLLDPE Film Envelope | Conventional Z-N LLDPE Film Envelope |
|---|---|---|---|
| Melt mass-flow rate | ISO 1133-1:2022 | 0.8–2.0 g/10 min | 0.8–2.0 g/10 min |
| Density | ISO 1183-1:2019 | 0.915–0.925 g/cm³ | 0.915–0.925 g/cm³ |
| Heat seal initiation | ASTM F88/F88M-15 | 85–105 °C | 95–115 °C |
| Haze on 50 µm blown film | ASTM D1003-13 | 2–6 % | 5–12 % |
| Dart drop impact | ASTM D1709-16a | higher by 20–40 % at equivalent density | baseline |
| Hexane extractables | ASTM D5227-13 | commonly <2.0 % | commonly <3.0 % |
On vertical form-fill-seal and flow-wrap lines, resin selection is often dominated by heat-seal behaviour. The more uniform branching distribution of mLLDPE can lower the seal initiation temperature by 5–12 °C relative to a conventional Z-N LLDPE of the same density. The practical result is an increase in sealing speed because the dwell time required to reach the seal plateau is reduced; however, the actual temperature offset is film-gauge and additive dependent. Hot-tack force is a critical property for vertical lines because the product load acts on the seal before full crystallization. ASTM F1921-12 provides a method for hot-tack measurement; a comparative curve should be generated at seal-bar temperatures from 90 °C to 150 °C and dwell times from 0.2 s to 1.0 s. Corona treatment to obtain a surface energy above 38 mN/m is frequently required before lamination or printing because mLLDPE films can have lower surface polarity and higher slip migration than some copolymers. Without in-line treatment, water-based inks and laminating adhesives may show wetting failure or delamination at the film interface. For frozen-food pouches, the combination of low-temperature toughness and seal integrity is often evaluated using ASTM D1709-16a and a filled-bag drop test; however, no single laboratory value predicts field performance across all converting lines.
Blocking is a known failure mode with uniform-chain mLLDPE films, especially when slip and antiblock loads are minimal or when mill rolls are stored above 35 °C. In high-speed VFFS operation, film-to-film friction must be controlled within a narrow band: too high, and the film cannot slide over forming collars; too low, and the film slips through the pull belts and loses registration. Coefficient of friction values measured by ASTM D1894-14 in the range of 0.20–0.30 are often targeted, but the appropriate value depends on the machine’s pull-belt pressure and forming geometry. Re-extrusion of edge trim and slit waste presents another boundary. mLLDPE film scrap can be added back at levels up to 20 % in some cast lines, but the loss of slip agent during processing and the formation of gel particles after repeated heat histories may increase. Fines and dust from grinding can reduce bulk density and cause feed-throat bridging; screening through a 2 mm mesh before return to the extruder is recommended. During start-up and shutdown, melt residence time must be managed. LLDPE resins degrade by thermo-oxidative chain scission and crosslinking when held at processing temperatures for extended periods; gelled specks on film are the visible signature. For narrow-MWD metallocene grades, purging with a material of similar viscosity before shutdown is preferred over high-viscosity purge compounds that may generate interfacial phase separation and line contamination. Outdoor storage of unprocessed pellets should be avoided unless the supplier confirms UV stabilisation in the BUE 5581 additive package; films exposed to sunlight can lose mechanical properties through photo-oxidation unless a UV stabiliser is included.
Food-contact compliance for Icorene 1761 BUE 5581 must be established through the supplier’s product stewardship documentation. In the United States, olefin polymers may be cleared under FDA 21 CFR 177.1520 provided the composition and conditions of use meet the specified extractives limits. In the European Union, Commission Regulation (EU) No 10/2011 requires demonstration that overall migration does not exceed 10 mg/dm² of food-contact surface area, or 60 mg/kg for infants and young children. For specific additives and monomers, the specific migration limits in the same regulation apply and must be checked against the formulation. REACH Regulation (EC) No 1907/2006 imposes registration and supply-chain communication duties; substances of very high concern above 0.1 % w/w in the article must be communicated. These requirements are not automatic properties of the resin; converter-specific validation is necessary because migration levels depend on film thickness, food simulant, time, and temperature.
| Region | Standard/Regulation | Typical Requirement for Polyethylene Film |
|---|---|---|
| United States | FDA 21 CFR 177.1520 | Olefin polymer clearance; extractives and end-use limitations apply |
| European Union | (EU) No 10/2011 | Overall migration limit 10 mg/dm²; 60 mg/kg for infant materials |
| European Union | REACH Regulation (EC) No 1907/2006 | Registration; SVHC communication above 0.1 % w/w |
Migration testing for specific applications should follow the time/temperature conditions of (EU) No 10/2011 using food simulants A, B, C, D1, D2, or E as appropriate. For fatty foods, simulant D2 or 95 % ethanol may be required. The film supplier should be consulted to confirm whether the full formulation is suitable for fatty-food contact and whether any limitation applies to high-temperature sterilization, microwave reheating, or long-term storage above 40 °C.