| HS Code | 986328 |
| Density | 0.918 g/cm³ |
| Melt Index | 1.0 g/10 min |
| Melt Flow Ratio | 30 |
| Tensile Strength At Yield | 10.3 MPa (MD) / 10.0 MPa (TD) |
| Tensile Strength At Break | 25.5 MPa (MD) / 22.0 MPa (TD) |
| Elongation At Break | 700% (MD) / 800% (TD) |
| Tensile Modulus | 0.207 GPa |
| Dart Drop Impact | 120 g |
| Elmendorf Tear Strength | 300 g (MD) / 400 g (TD) |
| Vicat Softening Point | 95 °C |
| Melting Point | 122 °C |
| Haze | 10% |
| Gloss | 70% |
As an accredited LyondellBasell Icorene 1210 NAT 0000 Polyethylene, Linear Low Density factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | LyondellBasell Icorene 1210 NAT 0000 Linear Low Density Polyethylene is supplied in 25 kg bags and 1,000 kg bulk bags. |
| Container Loading (20′ FCL) | 20′ FCL container loading: LyondellBasell Icorene 1210 NAT 0000 LLDPE in 25 kg bags, palletized, shrink-wrapped, and secured for safe transport. |
| Shipping | LyondellBasell Icorene 1210 NAT 0000 is a non-hazardous linear low-density polyethylene resin. It ships in 25 kg bags, bulk bags, or bulk trucks/railcars. No UN number, hazard class, or DOT/IMDG/IATA regulation applies. Store dry, sealed, away from heat, sunlight, and ignition sources. Handle as non-dangerous goods; avoid spills due to slip hazard. |
| Storage | Store LyondellBasell Icorene 1210 NAT 0000 in a cool, dry, well-ventilated warehouse at ambient temperature, away from direct sunlight, heat, flames, and strong oxidizers. Keep original packaging closed, palletized, and off the ground. Protect from moisture, dust, and contamination; avoid excessive stacking. Clean pellet spills promptly to prevent slipping, and follow the supplier’s SDS. |
| Shelf Life | Shelf life is 24 months when stored in original packaging in a cool, dry place away from direct sunlight. |
In stationary chemical containment applications, a linear low density polyethylene powder with a nominal density of 0.924 g/cm³ (ASTM D1505) and a melt flow rate of 10 g/10 min at 190°C/2.16 kg (ASTM D1238) is dry-charged into fabricated steel or cast aluminum molds on a carousel rotational molding line. The compliance framework for finished tanks includes ASTM D1998-21 for upright polyethylene storage tanks, FDA 21 CFR 177.1520 for olefin polymers in food contact, NSF/ANSI/CAN 61 for potable water system components, and EN 13341:2005+A1:2011 for static thermoplastic tanks for above-ground storage of domestic heating oils, lubricants, and other liquids; tanks intended for transport of dangerous goods fall under UN Model Regulations Chapter 6.5 for intermediate bulk containers, but this grade is more commonly associated with stationary installations. Single-layer tank formulations are processed at 100 wt% natural powder; dry-blended additives are metered at 0.2–1.0 wt% hindered amine light stabilizer, 0.1–0.5 wt% primary antioxidant, and 0.1–0.3 wt% carbon black for ultraviolet opacity where outdoor service is specified. The rotomolding process operates with oven set-point temperatures of 280–320°C, a peak internal air temperature of 190–220°C, biaxial rotation ratios near 4:1 for cylindrical tanks, and forced-air cooling followed by water mist at rates of 5–10°C/min. Field failures on carousel lines typically appear as localized thinning on the top pole of the mold when the rotation ratio deviates from 4:1, or as oxidative discoloration when internal air temperature exceeds 220°C for more than 5 min. Wall thickness ranges from 5 mm to 15 mm depending on hydrostatic head and tank profile; powder charge mass is calculated as the product of mold surface area, target wall thickness, and nominal melt density, divided by transfer efficiency. Terminal products include agricultural sprayer tanks, potable water storage tanks, chemical dosing tanks, diesel fuel tanks, and septic tank bodies. Operational boundaries are defined by the 0.924 g/cm³ density, which provides lower tensile yield strength than high-density polyethylene and reduces allowable wall stress in unsupported spans; chemical compatibility must be verified for each stored medium, and continuous service above 60°C with aggressive hydrocarbons or strong oxidizing acids is not recommended without fluorination or a multi-layer structure incorporating a crosslinked polyethylene inner layer.
For recreational watercraft and playground components molded with the same linear low density polyethylene powder, the peak internal air temperature window is constrained to 185–210°C because vertical wall sections in deep-draw multi-part molds begin to sag when the internal air exceeds 210°C, while incomplete bubble removal is observed below 185°C. The 10 g/10 min melt flow rate allows the material to penetrate ribs, inserts, and narrow mold channels at lower internal temperatures, but it also reduces melt strength relative to lower-melt-flow rotomolding grades. Equipment consists of carousel or shuttle rotational molding machines with cast aluminum molds, oven set-points of 260–300°C, rotation ratios near 5:1 for kayak hulls, forced-air cooling at approximately 25 m/s, and water mist at 20°C for dimensional stabilization. Compliance requirements include EN 1176-1:2017 and ASTM F1487-21 for playground equipment, ASTM F963-23 for toy-grade components, Directive 2013/53/EU for recreational craft where sit-on-top kayaks are concerned, and ISO 12215-4:2002 for small craft hull structural assessment. Dry-blend formulation addition ratios are: pigment 0.2–1.0 wt%, hindered amine light stabilizer 0.3–1.5 wt%, antioxidant 0.1–0.4 wt%, and metallic stearate mold release 0.1–0.3 wt%, with the balance being the linear low density polyethylene powder. Terminal products include sit-on-top kayak hulls, paddleboard bodies, playground slides, climbing holds, and sand-and-water play components. The operational limitation is that pigment loading above 1.5 wt% measurably reduces low-temperature impact strength; outdoor service requires a hindered amine light stabilizer package, and wall thickness tolerance in complex geometry typically falls within ±15% of nominal.
Following phosphating and degreasing of steel wire substrates, the fluidized-bed immersion process for linear low density polyethylene powder coating requires preheating the metal to 260–350°C, then dipping it into a fluidized bed with air pressure of 0.1–0.3 MPa for 3–10 s. The powder fuses on contact and is post-heated at 200–250°C for 2–5 min to level the surface, followed by water quenching. Coating thickness is controlled between 0.2 mm and 0.8 mm by adjusting preheat temperature and dip time; quench rate influences crystallinity and therefore impact resistance of the cooled coating. Compliance for food-contact wire goods includes FDA 21 CFR 175.300 for resinous and polymeric coatings, NSF/ANSI 51 for food equipment materials, RoHS Directive 2011/65/EU for restricted substances in electrical and electronic equipment, and REACH SVHC thresholds of 0.1 wt%. Formulation addition ratios for the powder compound are: linear low density polyethylene powder as the balance, pigment 1–5 wt%, flow modifier 0.5–2 wt%, adhesion promoter 0.5–3 wt%, and antioxidant 0.1–0.5 wt%. Terminal products include dishwasher baskets, refrigerator shelves, wire display racks, outdoor furniture, and protective-coated handrails. The process boundary is defined by adhesion: untreated steel with surface roughness below Ra 3 µm does not provide adequate mechanical anchoring, while coating thickness above 1.2 mm generates residual stress that leads to cracking at sharp wire intersections.
In masterbatch production, the linear low density polyethylene powder is used as a carrier resin because its melting range of 120–124°C (ASTM D3418) permits early pigment wetting in the twin-screw extruder before the high-shear dispersion zone. The process sequence begins with a high-speed mixer operating at 1,500–3,000 rpm for 5–10 min to coat pigment particles with the powder, followed by a co-rotating twin-screw extruder with L/D 40:1, screw speed 400–800 rpm, and barrel temperature profile 160–200°C. Strand pelletizing or underwater pelletizing is selected according to melt viscosity and pigment loading. Compliance matrices for masterbatch destined for food-contact packaging include EU 10/2011 with an overall migration limit of 10 mg/dm², FDA 21 CFR 177.1520 for olefin polymers under conditions B through H, ISO 11469 for polymer identification marking, and REACH SVHC concentration below 0.1 wt%. Formulation addition ratios are: carrier resin as the balance, pigment 30–60 wt%, dispersant 5–10 wt%, and processing aid 1–5 wt%. Terminal products include color masterbatch for blown film, injection molding, and rotational molding, as well as additive masterbatches for ultraviolet stabilization, slip, antistatic, and processing. The operational limitation is carrier-host viscosity mismatch: the 10 g/10 min melt flow rate may be significantly higher than the host resin, requiring let-down ratio adjustment to avoid dispersion defects in the final article.
| Standard | Scope | Clause/Test Method | Threshold/Limit |
|---|---|---|---|
| EU 10/2011 | Plastic materials and articles intended for food contact | Overall migration | 10 mg/dm² |
| FDA 21 CFR 177.1520 | Olefin polymers for food contact | Conditions B through H | Extractables per table |
| ISO 11469 | Polymer identification marking | Symbols and abbreviated terms | Marking code |
| REACH | Substances of very high concern | Candidate list declaration | 0.1 wt% |
When a linear low density polyethylene powder with a melt flow rate of 10 g/10 min is substituted for extrusion-coated films in carpet backing consolidation, the scattering process applies 200–500 g/m² of powder onto a polypropylene primary backing, followed by infrared or hot-air heating at 130–180°C for 30–90 s and lamination with a secondary backing through calender rolls at 2–5 bar. The melt viscosity of the powder at the lamination temperature governs tuft penetration depth and peel strength between the primary and secondary backings; loop pile constructions exhibit lower penetration depths than cut pile at the same coating weight. Published formulation data specific to this Icorene grade in carpet backing remains limited; the process parameters below represent general LLDPE powder behavior in tufted carpet lamination. Compliance requirements include FMVSS 302 for automotive interior flammability, ASTM D2859 for carpet flammability, EN 1307 for carpet classification, REACH SVHC limits of 0.1 wt%, and California Proposition 65 where applicable. Formulation addition ratios are: linear low density polyethylene powder 65–80 wt%, ethylene-vinyl acetate copolymer 10–20 wt% for flexibility, tackifier 5–10 wt%, and mineral filler 0–10 wt%, with the powder content reduced accordingly when filler is present. Terminal products include automotive floor carpets, entrance mats, carpet tiles, and acoustic insulation backing. The dominant process constraint is adhesion to untreated polypropylene: without corona or plasma treatment raising the surface energy above 42 mN/m, peel strength fails to meet automotive specification.
Competitive LyondellBasell Icorene 1210 NAT 0000 Polyethylene, Linear Low Density prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
LyondellBasell Icorene 1210 NAT 0000 is designated as a linear low density polyethylene resin supplied in natural form. The NAT 0000 suffix indicates that the lot is not pre-colored and does not contain a carbon black or pigmented masterbatch; any wide-spectrum ultraviolet stabilization required for outdoor service must be added downstream. The grade designation 1210 follows a producer code pattern in which the initial digits commonly signal a nominal melt flow rate near 12 g/10 min under ISO 1133-1:2022 or ASTM D1238-20 at 190 °C and 2.16 kg. Public disclosure of product-specific values is limited; therefore, nominal inference from the grade code should not replace the current LyondellBasell technical data sheet or certificate of analysis. Within the LLDPE class, density typically remains in the 0.910–0.925 g/cm³ envelope when measured by ASTM D792-20 or ISO 1183-1:2019, but the exact value for any production campaign may shift with comonomer type and conversion consistency.
For incoming lot verification, the melt mass-flow rate should be measured before production release because LLDPE lots can exhibit batch-to-batch melt-index drift of ±0.5 g/10 min or more around the target without altering the grade name. Density and volatile content should be checked according to ASTM D792-20 and ISO 15512:2019 or an equivalent Karl Fischer method when moisture-induced splay is observed. The natural pellet form may pick up surface water during humid transit; a hot-air hopper dryer at 80 °C for 2 h is usually sufficient when storage relative humidity exceeds 60 % RH. Published data for this specific configuration is limited, so the manufacturer’s recommended drying and processing conditions take precedence.
At the molecular level, LLDPE is a copolymer of ethylene and an alpha-olefin such as 1-butene, 1-hexene, or 1-octene. The comonomer introduces short-chain branches along an otherwise linear backbone, interrupting crystallinity and producing lamellae thinner than those in high density polyethylene. This architecture lowers density and modulus relative to HDPE while raising puncture resistance and environmental stress crack resistance. In a comparative selection, an LLDPE grade with a density near 0.912 g/cm³ and melt flow rate near 12 g/10 min typically shows lower tensile yield strength than a 0.950 g/cm³ HDPE but higher elongation at break and lower brittleness temperature. Testing should follow ISO 527-2:2012 or ASTM D638-14 for tensile properties, ASTM D790-17 for flexural modulus, and ASTM D256-10 or ISO 180:2023 for notched impact if the application requires it.
Dart impact and seal initiation are direct consequences of short-chain branching. Film made from LLDPE exhibits lower heat-seal initiation temperatures than high-pressure LDPE of similar density because the linear backbone and narrow composition distribution permit melting of thinner lamellae at lower temperatures; seal performance is measured with ASTM F2029-16 or ASTM F88/F88M-21. For injection-molded articles, the useful translation is impact toughness at low temperatures. The dart test ASTM D1709-16a is more relevant to film than to molded parts; for molded parts, instrumented puncture ISO 6603-2:2023 may be applied. Users should not extrapolate film dart values to injection-molded components without geometry-specific validation.
On injection molding lines with high-cavitation closure tools, the melt flow class suggested by the 1210 suffix allows filling of thin sections at lower packing pressures than a 0.5 g/10 min rotational molding grade, but the narrow melt-temperature window demands active temperature control. A general-purpose reciprocating screw with 20:1 or 24:1 L/D and a compression ratio of 2.5:1 to 3.5:1 is sufficient; barrier screws are preferred when venting is not available to avoid feed-throat plugging with regrind. Melt temperature should be verified with a needle pyrometer at the nozzle and compared against the barrel set points. For LLDPE grades with similar flow characteristics, a barrel profile from 170 °C at the feed section to 220 °C at the nozzle is typical, but the actual operating window may be as narrow as ±5 °C if the additive package has limited oxidative protection. Above 240 °C, oxidation can reduce the oxidation induction time measured by ASTM D3895-19 to less than 10 min and produce gelled specks or surface discoloration. Total residence time at melt temperature should not exceed 30 min; when downstream equipment stalls, barrel temperature should be lowered or the charge purged with an inert polymer such as a fractional-melt HDPE.
Mold cooling is a process conflict in LLDPE molding because fast solidification increases production rate but freezes molecular orientation that can raise anisotropic shrinkage. Mold temperatures from 10 °C to 40 °C are common for general-purpose LLDPE, and ejection temperatures should be below the Vicat softening point to avoid ejection marks. Shrinkage measured by ASTM D955-08 for similar injection-molding LLDPE grades typically falls between 0.015 mm/mm and 0.030 mm/mm along flow and can be 0.005–0.010 mm/mm higher transverse to flow, depending on gate design, packing time, and wall thickness. A holding-pressure profile with 0.5–2.0 s of gate-seal time per 1 mm of wall thickness minimizes sink marks; for a 2 mm sidewall, gate-seal verification should be performed by incrementing hold time until part mass stabilizes. Published data for this specific configuration is limited, so these values are class-level starting points rather than LyondellBasell-guaranteed settings.
Capillary rheometry is recommended for establishing the true shear-thinning envelope before designing multi-cavity hot-runner drop geometry. For LLDPE grades with melt flow rates around 12 g/10 min, apparent shear viscosity at 190 °C and 100 s⁻¹ is commonly in the range of 200–600 Pa·s, falling to 50–150 Pa·s at 1000 s⁻¹. These values are not specific to Icorene 1210 NAT 0000 but illustrate why LLDPE fills thin sections more easily than a 4 g/10 min grade at identical pressure. The shear viscosity should be measured according to ISO 11443:2021 using a capillary die of 1 mm diameter and 20:1 length-to-diameter ratio; end corrections should follow the Bagley procedure. Entrance pressure loss is lower than for HDPE at equivalent melt index because the shear-thinning slope of LLDPE is more gradual; however, melt strength is lower than LDPE, so thick-wall parts can sag in the mold during cooling if injection speed is too slow.
On production-scale equipment, a recurrent failure mode in natural LLDPE is splay caused by volatiles or moisture at the feed throat. If regrind contains dust or static-charged fines, the use of a vented barrel without vacuum can cause vent plugging. A three-zone screw with a 20:1 L/D may generate insufficient melt homogeneity for thin-wall parts, leading to flow marks near the gate. In such cases, a barrier screw or a mixing nozzle with a 40–60 mesh screen pack can improve surface quality, but melt temperature must then be compensated by 5–10 °C to offset pressure rise. Clamp force requirement for a multi-cavity LLDPE tool can be approximated from the projected cavity area; a 1500 kN toggle-clamp machine may be adequate for a 200 cm³ shot of LLDPE at 50 MPa average cavity pressure, but hot-runner pressure losses must be included. Published data for this specific configuration is limited, so mold trial validation is necessary.
Natural unfilled LLDPE lots require a defined incoming inspection protocol because the absence of colorant exposes contamination and yellowing that may be hidden in black or heavily pigmented compounds. The melt flow rate should be measured according to ISO 1133-1:2022 using condition 190/2.16; density should be measured after conditioning for 24 h at 23 °C and 50 % RH using ISO 1183-1:2019 Method A or ASTM D792-20 Method B. Tensile yield stress and elongation at break are determined at 50 mm/min with ISO 527-2:2012 Type 1A specimens or at 50 mm/min with ASTM D638-14 Type IV specimens. Flexural modulus, where required for lid stiffness, is measured by ISO 178:2019 or ASTM D790-17 at 2 mm/min. Vicat softening temperature should be measured by ISO 306:2022 Method A50 or ASTM D1525-17e1 using a 10 N load and 50 °C/h ramp. For food-contact use, the resin supplier should confirm compliance with 21 CFR 177.1520 and EU 10/2011; the natural grade’s regulatory status depends on catalyst residues, comonomer type, and antioxidant package. The grade should be classified under ISO 1872-1:2018 when included in ISO-based polyethylene specifications.
Thermal characterization by differential scanning calorimetry can establish the melting peak and crystallinity for lot-to-lot comparison. LLDPE grades with density below 0.920 g/cm³ often show a broad melting endotherm with peak temperature near 120–125 °C at 10 °C/min heating rate according to ASTM D3418-21 or ISO 11357-3:2018; the presence of a second, high-temperature shoulder may indicate high-density contamination or poor comonomer distribution. Oxidation induction time should be tested as part of new-source qualification but is not a routine check for all molding operations. If yellowing occurs in natural parts, the root cause may be antioxidant depletion, excessive residence time, or mold release chemistry; elemental analysis and melt-flow stability after multiple extrusions can isolate the cause.
Comparative selection against high-pressure low density polyethylene and high density polyethylene should be based on the solid-state failure mode, not only on nominal density. High-pressure LDPE has long-chain branching, broader molecular weight distribution, and lower melt flow activation energy, which improves neck-in and bubble stability in extrusion but reduces tensile strength and puncture resistance relative to LLDPE at equivalent density. HDPE offers higher flexural modulus and Vicat softening, but the lower comonomer content reduces slow crack growth resistance, making it less suitable for snap-fit closures that experience repeated bending. LLDPE produces lower warpage in flat thin-wall parts than some HDPE grades due to lower crystal growth rate, but the same property can increase cycle time if mold temperature is insufficiently cooled. For applications such as closures, thin-wall containers, and housewares in the 12 g/10 min flow class, LLDPE grades can fill multi-cavity tools at moderate injection pressures while retaining ductile failure in cold conditions.
| Property | ASTM/ISO method | LLDPE range | LDPE range | HDPE range |
|---|---|---|---|---|
| Density | ASTM D792-20 / ISO 1183-1:2019 | 0.910–0.925 g/cm³ | 0.915–0.932 g/cm³ | 0.940–0.965 g/cm³ |
| Melt flow rate | ISO 1133-1:2022 / ASTM D1238-20 | 5–25 g/10 min injection grades | 0.2–75 g/10 min | 0.2–30 g/10 min |
| Tensile yield strength | ISO 527-2:2012 / ASTM D638-14 | 7–14 MPa | 6–12 MPa | 17–30 MPa |
| Elongation at break | ISO 527-2:2012 / ASTM D638-14 | 700–1000 % | 100–700 % | 100–1000 % |
| Dart impact | ASTM D1709-16a | 200–1000 g | 50–200 g | 100–400 g |
| Environmental stress crack resistance | ASTM D1693-15b | 100–1000 h | 10–100 h | 10–1000 h |
| Vicat softening temperature | ASTM D1525-17e1 / ISO 306:2022 | 80–105 °C | 70–100 °C | 115–135 °C |
Compared with ultralow density polyethylene or plastomer grades produced with metallocene catalysts, this LLDPE class generally has higher crystallinity and less clarity. If the application requires glass-like clarity in blown film or injection-molded parts, a metallocene LLDPE or a suitable propylene-ethylene random copolymer may be more appropriate. The Ziegler-Natta or chromium-catalyzed low-pressure process class can produce a broader comonomer distribution, which improves low-temperature impact by tying thicker lamellae to amorphous tie chains, but reduces peak melting sharpness. Product-specific production technology for Icorene 1210 NAT 0000 is not publicly specified in available literature; therefore, comparisons must be made from thermal and rheological testing rather than from catalyst chemistry assumptions.
When this resin is used outdoors without UV stabilization, surface chalking and loss of elongation are expected; the natural grade should not be considered a weatherable grade unless a hindered amine light stabilizer package is added at the recommended loading and validated by ASTM G154-23 or ISO 4892-3:2024. Storage in direct sunlight or high-temperature containers can consume the antioxidant package prematurely. Avoid blending with ionomers, EVOH, or polyamides without adequate compatibilization when high scrap recovery is planned; layer boundaries or domain interfaces may produce delamination at gate vestiges. Processing of regrind should be limited to 20–30 % by weight for visible natural parts unless the operation verifies melt-flow retention, color, and impact properties after each recycle pass. The natural form also lacks slip and antiblock additives unless specified in the grade documentation; high-speed filling equipment may require external lubrication or additive masterbatch to maintain part release.